A method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and reusing it in lithium manganate secondary batteries

By combining physical and chemical separation technology in waste alkali zinc-manganese batteries, and preparing lithium manganese materials through high-temperature solid phase method, the complex and application limitations of waste zinc-manganese batteries are solved, and high efficiency is achieved , The preparation of low-pollution lithium manganate battery positive electrode material has significant economic and social benefits.

CN114843539BActive Publication Date: 2024-11-08NINGBO INST OF TECH ZHEJIANG UNIV ZHEJIANG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210537918.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-17
Publication Date
2024-11-08
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

The prior art has complex processes and a lot of pollution in the recycling of waste zinc-manganese batteries. The application of manganese dioxide is relatively limited in lithium-ion batteries, and it has not fully utilized its resource value.

Method used

Manganese dioxide is extracted from waste alkaline zinc-manganese dry batteries by using wet recycling technology combined with physical separation and chemical separation, and high-purity lithium manganese material is prepared by high-temperature solid phase method for the positive electrode material of lithium-ion batteries.

Benefits of technology

It has achieved high added value utilization with simple process, low pollution and high recovery rate. Lithium manganate batteries show high specific capacity and cycle stability. They are suitable for lithium-ion batteries and have important economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114843539B_ABST
    Figure CN114843539B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and using the same to prepare lithium manganate secondary batteries. The method collects carbon bags from alkaline zinc-manganese batteries and adopts a wet recovery technology combining impurity removal, reduction, precipitation and calcination to obtain manganese dioxide. e ‑MnO2, and react with lithium hydroxide by high-temperature solid phase method to obtain the final product - high-purity lithium manganate, which can be used as a high-performance lithium-ion battery positive electrode material. The advantages of the present invention are: the experimental conditions of the process are easy to control, the raw materials are cheap and widely available, the required reagents and instruments are common and cheap, and it has extremely high feasibility in both technology and economy. The prepared lithium manganate has extremely high specific capacity and cycle stability, and achieves a win-win situation for environmental protection and economy from the two aspects of solid waste recycling and low-carbon economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of resource recycling and battery technology, in particular to a method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and applying the manganese dioxide to lithium manganate secondary batteries. Background Art

[0002] Waste zinc-manganese batteries contain heavy metals such as mercury, cadmium, zinc, copper, and manganese. If discarded at will, it will pollute the environment and waste metal resources. my country scraps 500,000 tons of waste zinc-manganese batteries every year. If all of them can be recycled, 110,000 tons of manganese, 70,000 tons of zinc, and 14,000 tons of copper can be recycled, which can generate considerable economic and social benefits.

[0003] At present, the recycling process of zinc-manganese dry batteries that have been industrialized abroad is mostly a pyrometallurgical process. This process first removes mercury from the dry batteries by roasting, and then enters the ore-fired electric furnace to smelt slag, ferromanganese and zinc. At the same time, this process can also realize the closed-loop circulation of sludge and CO waste gas, reducing secondary pollution. It is reported that Germany has now achieved the collection, classification and disposal of all waste batteries, and all kinds of highly toxic batteries are marked with recycling logos, strictly requiring manufacturers and buyers to classify and recycle batteries, and strictly managing the recycling and processing equipment of battery manufacturers. Researchers at the Aachen University of Technology in Germany use waste zinc-manganese dry batteries as raw materials, pyrolyze or crush them, and screen manganese powder and carbon black after crushing to make balls. After that, the pyrolyzed batteries and pellets are put into the direct current ore-fired furnace (DC-SAF) for smelting to obtain ferromanganese alloy and zinc oxide powder. At present, the process has completed the laboratory stage research work and achieved good results.

[0004] Although China started relatively slowly in recycling, it has now achieved many research results. Zhao Dongjiang et al. used wet recycling technology to prepare MnCO3 using recycled waste zinc-manganese dry batteries as raw materials. The experimental results show that the yield of MnCO3 is mainly affected by the concentration, volume and soaking time of the acid during acid leaching. The yield of MnCO3 can reach 63.76%. Kong Xiangping used waste alkaline zinc-manganese dry batteries as raw materials, roasted carbon powder, acid-leached metal zinc and manganese in carbon powder, and then added Na2CO3 to generate MnCO3. MnO2 was obtained by high-temperature decomposition of MnCO3 powder. The experimental results show that the manganese recovery rate can be as high as 93.2%. Cheng Jianliang et al. treated waste zinc-manganese dry batteries at high temperature, then soaked them in H2SO4 to obtain manganese, zinc and iron ions, and finally used (NH4)2C2O4 as a precipitant to prepare manganese-zinc ferrite by co-precipitation, and characterized the samples by XRD and SEM. The results show that the obtained zinc-manganese ferrite has good structure and morphology, and is at the micron level.

[0005] At present, although there are many studies on the recovery of manganese dioxide from waste zinc-manganese batteries in China, most of the processes are relatively complicated and difficult to scale up. At the same time, the application of recycled manganese dioxide is also relatively limited, especially its reuse in lithium-ion batteries has rarely been reported. At present, the annual output value of lithium-ion batteries in the world exceeds 200 billion yuan, of which my country accounts for more than 40%. Therefore, the manganese dioxide extracted from waste dry batteries as an important raw material has great development potential for application in lithium-ion battery materials. Summary of the invention

[0006] The purpose of the present invention is to provide a new method for extracting valuable materials from waste dry batteries. The method comprises collecting the carbon bags of alkaline zinc-manganese dry batteries and adopting a wet recovery technology combining physical separation and chemical separation to obtain valuable materials. ε -MnO2, and use high-temperature solid phase method to produce high-purity lithium manganate material, which can be used as positive electrode material for lithium-ion batteries to achieve high added value. Compared with traditional recycling methods, this method has the advantages of novel method, simple process, low pollution and high recovery rate.

[0007] The technical solution of the present invention:

[0008] The present invention provides a method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and recycling it in lithium manganate batteries. The lithium manganate product obtained by chemically removing impurities and high-temperature calcining the carbon bag in the waste alkaline zinc-manganese dry batteries has extremely high specific capacity and cycle stability, thereby realizing high added value utilization of waste solids.

[0009] A method for preparing a lithium manganate secondary battery by extracting manganese dioxide from waste alkaline zinc-manganese dry batteries for reuse, characterized in that it comprises the following steps:

[0010] (1) Extraction of manganese: Collect the carbon bag of alkaline zinc-manganese battery, and obtain MnCO3 crystals by impurity removal, reduction and precipitation;

[0011] (2) Preparation of manganese dioxide: Take the MnCO3 crystals from step (1) and calcine them at high temperature to obtain a black product. ε -MnO2 crystals;

[0012] (3) Preparation of lithium manganate: Take the ε -MnO2 crystals are reacted with lithium hydroxide by a high-temperature solid phase method to prepare high-purity lithium manganate, namely LiMn2O4 crystals;

[0013] (4) Preparation of positive electrode of battery: Take the LiMn2O4 crystals of step (3) and mix them with appropriate amount of binder and conductive carbon, add dispersant and stir to obtain black slurry, evenly apply it on the surface of aluminum foil, vacuum dry and cut to obtain positive electrode sheet;

[0014] (5) Assembly and testing of lithium manganese oxide: The lithium manganese oxide electrode prepared in step (4) is used as the positive electrode, metallic lithium is used as the negative electrode of the battery, the electrolyte lithium hexafluorophosphate is used as the electrolyte, and the commercial polypropylene (PP) film is used as the battery separator to assemble a button cell, that is, a lithium manganese oxide secondary battery.

[0015] A method for preparing a lithium manganate secondary battery by extracting manganese dioxide from waste alkaline zinc-manganese dry batteries for reuse, characterized in that it comprises the following steps:

[0016] (1) Extraction of manganese: Mechanically disassemble the waste alkaline zinc-manganese dry batteries and collect the carbon bags; add water to dissolve the carbon bags to remove soluble electrolytes including NH4Cl and sodium salts; add sulfuric acid or hydrochloric acid to dissolve and remove metallic zinc; add H2SO4 or HCl and FeSO4 or KI or H2C2O4 or H2O2 or Na2S for acidic reduction, remove insoluble substances including C and SiO2 by suction filtration to obtain an acidic MnSO4 or MnCl2 solution; heat the solution until no bubbles are generated, add sufficient NH4HCO3 or NaHCO3 or Na2CO3 or K2CO3 to obtain a white MnCO3 crystal precipitate;

[0017] (2) Preparation of manganese dioxide: Take the MnCO3 crystals obtained in step (1), dry them, grind them into fine powder, place them in a tube furnace, and calcine them at high temperature in an air atmosphere to obtain ε -MnO2 crystals;

[0018] (3) Preparation of lithium manganate: Take the ε -MnO2 crystals, add a certain amount of LiOH, grind and mix, place in a tube furnace, calcine at high temperature in an air atmosphere, and cool naturally to room temperature to obtain spinel LiMn2O4 crystals;

[0019] (4) Preparation of positive electrode of battery: Grind the LiMn2O4 crystal obtained in step (3), mix with appropriate amount of binder and conductive carbon, add dispersant and stir to obtain black slurry, evenly apply it on the surface of aluminum foil, vacuum dry, and cut to obtain positive electrode sheet;

[0020] (5) Assembly and testing of lithium manganese oxide: The lithium manganese oxide electrode prepared in step (4) is used as the positive electrode, metallic lithium is used as the negative electrode of the battery, the electrolyte lithium hexafluorophosphate is used as the electrolyte, and the commercial polypropylene (PP) film is used as the battery separator to assemble a button battery, i.e., a lithium manganese oxide secondary battery.

[0021] The method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and using it in lithium manganate batteries comprises the following steps:

[0022] (1) Extraction of manganese: Mechanically disassemble the waste alkaline zinc-manganese batteries and collect the carbon bags. Dissolve the carbon bags in water to remove soluble electrolytes such as NH4Cl and sodium salts; add sulfuric acid or hydrochloric acid to dissolve and remove a small amount of metallic zinc; add H2SO4 or HCl and FeSO4 or KI or H2C2O4 or H2O2 or Na2S for acidic reduction to remove insoluble substances such as C and SiO2 to obtain an acidic MnSO4 or MnCl2 solution. Heat the solution until no bubbles are generated, add sufficient NH4HCO3 or NaHCO3 or Na2CO3 or K2CO3 to obtain a white precipitate.

[0023] (2) Preparation of manganese dioxide: The MnCO3 solid obtained in step (1) is ground, placed in a tube furnace, and calcined at high temperature in an air atmosphere to obtain a black product.

[0024] (3) Preparation of lithium manganate: The lithium manganate obtained in step (2) ε -MnO2 and a certain proportion of LiOH are fully ground and mixed, placed in a tube furnace, calcined at high temperature in an air atmosphere, and naturally cooled to room temperature to obtain a dark brown powder.

[0025] Furthermore, the method performs XPS elemental analysis on the samples obtained in steps (1), (2), and (3).

[0026] Furthermore, by adopting steps (1) and (2) of the present method, 5.87 g of ε -MnO2, 5.59 g of LiMn2O4 crystals can be obtained through step (3).

[0027] (4) Preparation of lithium manganese oxide positive electrode sheet: LiMn2O4 spinel is fully ground and mixed with an appropriate amount of binder and conductive carbon, and an appropriate amount of NMP dispersant is added. The mixture is stirred for 0.5 h to obtain a black slurry with a certain viscosity. The slurry is evenly coated on the surface of aluminum foil, vacuum dried, and then cut into electrode discs as positive electrode sheets for lithium manganese oxide batteries.

[0028] (5) Assembly and testing of lithium manganese oxide battery: The lithium manganese oxide electrode prepared in step (4) is used as the positive electrode, metal lithium is used as the negative electrode of the battery, commercial electrolyte lithium hexafluorophosphate is used as the electrolyte, and commercial polypropylene (PP) film is used as the battery separator. The button battery is assembled in a glove box with an argon atmosphere. The prepared battery is subjected to rate tests at different current densities and constant current cycle charge and discharge tests at different rates.

[0029] The battery recovered in step (1) is an alkaline zinc-manganese battery, whose shape includes but is not limited to cylindrical and rectangular, and whose size includes but is not limited to 5 and 7 batteries; the sulfuric acid concentration is 2 to 5 mol·L -l(The concentration of hydrochloric acid is doubled), the concentration of FeSO4 or KI or H2C2O4 or H2O2 or Na2S is 8-10 mol·L -1 .

[0030] The calcination temperature in step (2) is 300-500° C., and the calcination time is 1-6 h.

[0031] In step (3) n (MnO2): n (LiOH·H2O) is 2:1~2:1.5, the calcination temperature is 300~900 ℃, and the calcination time is 3~20 h.

[0032] The binder in step (4) is PVDF (polyvinylidene fluoride), the conductive carbon is acetylene black, the dispersion solvent is NMP (N-methylpyrrolidone), and m (LiMn2O4): m (PVDF): m (acetylene black) is 10:1:1~5:1:1, the drying temperature is 50~100 ℃, the time is 1~2 h, and the electrode sheet diameter is 10~15 mm.

[0033] The commercial electrolyte lithium hexafluorophosphate in step (5) contains ethylene carbonate and dimethyl carbonate. v (Ethylene carbonate): v (dimethyl carbonate) is 1:1, the lithium negative electrode is a lithium sheet, and the assembled button batteries include but are not limited to CR2016 and 2025 types.

[0034] Advantages of the present invention: In view of the problems of complex process, high equipment requirements and high pollution in the traditional waste battery recycling method of separating and smelting different metals or metal compounds in the battery for recycling, the present invention proposes a new recycling idea, in which the lithium manganese oxide product obtained by chemically removing impurities and high-temperature calcination of the carbon bag of the waste alkaline zinc-manganese battery is reused as the positive electrode material of the lithium ion battery. Therefore, the process is relatively simple, the cost is low, and it has extremely high feasibility in both technology and economy, and it has important practical value in the field of waste zinc-manganese battery treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 XRD pattern of MnCO3.

[0036] Figure 2 SEM (a) and high-resolution SEM (b) images of MnCO3.

[0037] Figure 3 XRD pattern of MnO2.

[0038] Figure 4SEM (a) and high-resolution SEM (b) images of MnO2.

[0039] Figure 5 XRD pattern of LiMn2O4.

[0040] Figure 6 SEM (a) and high-resolution SEM (b) images of LiMn2O4.

[0041] Figure 7 TEM (a) and high-resolution TEM (b) images of LiMn2O4.

[0042] Figure 8 XPS spectra of MnCO3, MnO2, and LiMn2O4.

[0043] Fig. 9 The charge and discharge curve of LiMn2O4 battery after 400 cycles of constant current at 1C rate.

[0044] Fig.10 The charge and discharge curve of LiMn2O4 battery after 400 cycles of constant current at 3C rate.

[0045] Fig.11 The charge and discharge curve of LiMn2O4 battery after 400 cycles of constant current cycling at 5C rate.

[0046] Fig.12 Actual working effect of LiMn2O4 battery LDE lamp at room temperature. DETAILED DESCRIPTION

[0047] In order to further clarify the present invention, preferred embodiments of the present invention will now be described. It should also be understood that the embodiments are provided for illustrative purposes and not to limit the scope of the present invention.

[0048] Example 1 Extraction and characterization of manganese:

[0049] Extraction of manganese: Mechanically disassemble the waste alkaline zinc-manganese batteries and collect the carbon bags. Dissolve the carbon bags in water to remove soluble electrolytes such as NH4Cl and sodium salts; add sulfuric acid or hydrochloric acid to dissolve and remove a small amount of metallic zinc; add H2SO4 or HCl and FeSO4 or KI or H2C2O4 or H2O2 or Na2S for acidic reduction to remove insoluble substances such as C and SiO2 to obtain acidic MnSO4 or MnCl2 solution. Heat the solution until no bubbles are generated, add sufficient NH4HCO3 or NaHCO3 or Na2CO3 or K2CO3 to obtain a white precipitate.

[0050] Characterization results: see Figure 1 and Figure 2 The dried white solid was analyzed by XRD ( Figure 1) shows that its structure is consistent with the PDF card (44-1472) and belongs to MnCO3 crystal. Figure 2 The SEM electron microscope image shows that its morphology is a spherical structure of 1 to 5 microns composed of particles of 10 to 20 nanometers.

[0051] Example 2: Preparation and characterization of manganese dioxide:

[0052] The MnCO3 solid obtained in Example 1 was ground, placed in a tube furnace, and calcined at high temperature in an air atmosphere to obtain a black product.

[0053] Characterization results: see Figure 3 ,and Figure 4 , XRD analysis ( Figure 3 ) shows that its structure is consistent with the PDF card (44-0141), belonging to ε -MnO2 crystals. Figure 4 The SEM electron microscope image shows that its morphology is a spherical structure of 1 to 5 micrometers composed of particles of 10 to 20 nanometers, which is similar to the MnCO3 crystals obtained in Example 1.

[0054] Example 3: Preparation of lithium manganate:

[0055] The obtained in Example 2 ε -MnO2 and a certain proportion of LiOH are fully ground and mixed, placed in a tube furnace, calcined at high temperature in an air atmosphere, and naturally cooled to room temperature to obtain a dark brown powder, namely LiMn2O4 crystals.

[0056] Characterization results: see Figures 5 to 7 , after XRD analysis ( Figure 5 ), showing that its structure is consistent with the PDF card (53-1237), belonging to the spinel LiMn2O4 crystal. Figure 6 The SEM electron microscope image shows that its morphology is a spinel structure of 50 to 200 nanometers, which is different from that in Example 2. ε -MnO2 is significantly different. Further, the spinel structure of LiMn2O4 crystals was verified by TEM analysis, such as Figure 7 shown.

[0057] Example 4: XPS elemental analysis of samples from Examples 1-3

[0058] XPS elemental analysis was performed on the samples obtained in Examples 1-3, and the energy spectra thereof were as follows: Figure 8 The corresponding element compositions are shown in Table 1.

[0059] Table 1

[0060] Mn (at.%) O (at.%) Li (at.%) <![CDATA[MnCO3]]> 20 80 -- <![CDATA[MnO2]]> 30 70 -- <![CDATA[LiMn2O4]]> 23 62 15

[0061] Experimental results: The XPS results show that the products prepared by the present invention are of high purity and free of other heteroatoms.

[0062] Example 5: Assembly of lithium manganate secondary battery:

[0063] Take the LiMn2O4 crystals prepared in Example 3, grind and mix them with appropriate amounts of binder and conductive carbon, add appropriate amounts of NMP dispersant, and stir for 0.5 h to obtain a black slurry with a certain viscosity. Apply it evenly to the surface of aluminum foil, vacuum dry it, and cut it into electrode discs as positive electrode sheets for lithium manganese oxide batteries; use the lithium manganese oxide electrode as the positive electrode sheet, metallic lithium as the negative electrode of the battery, commercial electrolyte lithium hexafluorophosphate as the electrolyte, and polypropylene (PP) film as the battery separator in a glove box with an argon atmosphere to obtain a button battery, i.e., a lithium manganese oxide secondary battery.

[0064] Example 6: Working performance test of lithium manganese oxide secondary battery:

[0065] The button battery prepared in Example 5 was subjected to a cycle performance test by charging and discharging for 400 cycles at a current of 1C (the current density required to fully charge the battery in 1 hour). The results are as follows: Fig. 9 shown.

[0066] The results show that the battery has a discharge capacity of 112 mAh / g at 1C current, and after 400 cycles, its capacity can still be maintained at 100 mAh / g, with a capacity loss of only 10%, showing excellent cycle performance. Furthermore, its Coulomb ratio charge and discharge efficiency can reach almost 100%.

[0067] Example 7: Working performance test of lithium manganate secondary battery:

[0068] The button battery prepared in Example 5 was subjected to a cycle performance test by charging and discharging for 400 cycles at a current of 3C (the current density required to fully charge the battery in 1 / 3 hour). The results are as follows: Fig.10 shown.

[0069] The results show that the battery has a discharge capacity of 91 mAh / g at 3C current, and after 400 cycles, its capacity can still be maintained at 86 mAh / g, with a capacity loss of only 5%, demonstrating excellent cycle performance at higher rates. Furthermore, its Coulomb ratio charge and discharge efficiency is close to 100%.

[0070] Example 8: Working performance test of lithium manganese oxide secondary battery:

[0071] The button battery prepared in Example 5 was subjected to a cycle performance test by charging and discharging for 400 cycles at a high current of 5C (the current density required to fully charge the battery in 1 / 5 hour). The results are as follows: Fig.11 shown.

[0072] The results show that the battery has a discharge capacity of 87 mAh / g at 5C current, and after 400 cycles, its capacity can still be maintained at 81 mAh / g, with a capacity loss of only 7%, showing excellent cycle performance under fast charging conditions. Furthermore, its Coulomb ratio charge and discharge efficiency is also close to 100%.

[0073] Example 9: Operating temperature test of lithium manganese oxide secondary battery

[0074] The button cell prepared in step (5) was charged, and its operating voltage was about 4.1 V. The battery can be used to light up the LED lamp at room temperature. Fig.12 shown.

[0075] The results show that the battery has good working performance at room temperature and can be used in practical scenarios.

Claims

1. A method for preparing a lithium manganate secondary battery by extracting manganese dioxide from waste alkaline zinc-manganese dry batteries for reuse, characterized in that: The following steps are involved: (1) Extraction of manganese: Mechanically disassemble the waste alkaline zinc-manganese dry batteries and collect the carbon bags; add water to dissolve the carbon bags to remove soluble electrolytes including NH4Cl and sodium salts; add sulfuric acid or hydrochloric acid to dissolve and remove metallic zinc; add H2SO4 or HCl and FeSO4 or KI or H2C2O4 or H2O2 or Na2S for acidic reduction, remove insoluble substances including C and SiO2 by suction filtration to obtain an acidic MnSO4 or MnCl2 solution; heat the solution until no bubbles are generated, add sufficient NH4HCO3 or NaHCO3 or Na2CO3 or K2CO3 to obtain a white MnCO3 crystal precipitate; (2) Preparation of manganese dioxide: Take the MnCO3 crystals obtained in step (1), dry them, grind them into fine powder, place them in a tube furnace, and calcine them at high temperature in an air atmosphere to obtain ε -MnO2 crystals; (3) Preparation of lithium manganate: Take the ε -MnO2 crystals, add a certain amount of LiOH, grind and mix, place in a tube furnace, calcine at high temperature in an air atmosphere, and cool naturally to room temperature to obtain spinel LiMn2O4 crystals; (4) Preparation of positive electrode of battery: Grind the LiMn2O4 crystal obtained in step (3), mix with appropriate amount of binder and conductive carbon, add dispersant and stir to obtain black slurry, evenly apply it on the surface of aluminum foil, vacuum dry, and cut to obtain positive electrode sheet; (5) Assembly and testing of lithium manganese oxide: The lithium manganese oxide electrode prepared in step (4) is used as the positive electrode, metallic lithium is used as the negative electrode of the battery, the electrolyte lithium hexafluorophosphate is used as the electrolyte, and the commercial polypropylene (PP) film is used as the battery separator to assemble a button battery, i.e., a lithium manganese oxide secondary battery.

2. The method for preparing a lithium manganate secondary battery according to claim 1, wherein: The battery recovered in step (1) is an alkaline zinc-manganese dry battery, which has a cylindrical or rectangular shape and a size of 5 or 7 batteries; the sulfuric acid concentration is 2 to 5 mol·L -l , or hydrochloric acid concentration of 4 to 10 mol·L -l , FeSO4 or KI or H2C2O4 or H2O2 or Na2S concentration is 8~10 mol·L -1 .

3. The method for preparing a lithium manganate secondary battery according to claim 1, wherein: In the step (2), the calcination temperature is 300-500°C and the calcination time is 1-6 hours.

4. The method for preparing a lithium manganate secondary battery according to claim 1, wherein: In the step (3), the molar ratio of MnO2 to LiOH·H2O is 2:1 to 2:1.5, the calcination temperature is 300 to 900°C, and the calcination time is 3 to 20 hours.

5. The method for preparing a lithium manganate secondary battery according to claim 1, wherein: The binder in step (4) is PVDF (polyvinylidene fluoride), the conductive carbon is acetylene black, the dispersing solvent is NMP (N-methylpyrrolidone), and the mass ratio of LiMn2O4, PVDF, and acetylene black is 10:1:1 to 5:1:

1. The drying temperature is 50 to 100°C, the time is 1 to 2 h, and the electrode sheet diameter is 10 to 15 mm.

6. The method for extracting manganese dioxide from waste alkaline zinc-manganese dry batteries and reusing them in lithium manganate secondary batteries as claimed in claim 1, characterized in that: The electrolyte lithium hexafluorophosphate in step (5) contains ethylene carbonate and dimethyl carbonate, and the volume ratio of ethylene carbonate to dimethyl carbonate is 1:

1. The negative electrode of the battery is a lithium sheet, and the assembled button batteries include CR2016 and 2025 types.

7. A lithium manganate secondary battery prepared by the method according to any one of claims 1 to 6.

8. A positive electrode of a lithium manganese oxide secondary battery, characterized in that: The method is prepared by the method according to any one of claims 1 to 6.

9. Use of the positive electrode as claimed in claim 8 in preparing a lithium manganate secondary battery.