A bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte material and preparation method thereof
Through bismuth-doped lithium germanium phosphorus and sulfur solid electrolyte material, the problems of low conductivity and poor chemical stability of lithium sulfide solid electrolyte materials are solved, high conductivity and good cycling performance are achieved, and it is suitable for all-solid lithium batteries, reducing the Cost and simplify the preparation process.
Patent Information
- Application Number
- CN202210486959.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-05-06
AI Technical Summary
The ionic conductivity of existing lithium-sulfur solid electrolyte materials is not high enough and the chemical stability is poor, resulting in the comprehensive performance of all-solid lithium batteries that cannot meet application needs and are costly.
The lithium germanium phosphorus and sulfur solid electrolyte material is made of bismuth doped with the chemical formula of LixGe1-yBiyP2S12. By replacing CeS2 as Bi2S3, the stoichiometric ratio and ball milling, pressing, heating and calcining steps are optimized to form a material with high conductivity and good chemical stability. .
It achieves high conductivity and good chemical stability, improves the mobility of lithium ions and the circulation performance of materials, reduces the stability of lithium metal, and simplifies the preparation process, and is suitable for all-solid-state lithium secondary batteries.
Smart Images

Figure CN114914527B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium-ion batteries, and specifically relates to a bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material and a preparation method thereof, which has good mechanical properties, excellent ionic conductivity, and good electrochemical stability, and can be used in all-solid-state lithium batteries. Background Art
[0002] Lithium-ion batteries have currently occupied the electric vehicle market in my country and are also being used on a large scale in the grid energy storage market. Battery technology is one of the key technologies to solve the current energy problem. In electric vehicles, energy density is the first indicator of power battery performance, while energy storage batteries pay more attention to cost and safety. With the growth of electric vehicle sales, the frequency of safety accidents such as electrolyte leakage, spontaneous combustion and explosion has also increased significantly, and energy storage power stations have also experienced many safety accidents. Safety issues have become a key issue hindering the further application and development of lithium-ion batteries. The main reason for the safety problem is that flammable organic electrolytes are used in lithium-ion batteries, which participate in combustion and release a large amount of heat when the battery has a short-circuit thermal runaway. All-solid-state batteries use solid electrolytes for ion conduction. Compared with traditional liquid batteries, they are non-flammable and non-volatile, and the safety of the battery has been greatly improved. Therefore, they have received widespread attention from academia and industry and are considered to be one of the most promising next-generation lithium-ion battery technologies.
[0003] Solid electrolytes are the core materials of all-solid-state batteries. Most of the current solid electrolytes have low ion conductivity, unstable electrochemical window and various interface problems. These problems make the comprehensive performance of current all-solid-state batteries unable to meet the application requirements, and there are no commercial products that can be launched. (There are some semi-solid commercial products.) Among the inorganic solid electrolytes reported so far, sulfide electrolytes have attracted much attention because of their highest ionic conductivity and good mechanical properties. However, the disadvantage of lithium-sulfur systems such as Li2S and P2S5 is that they are easily hydrolyzed and oxidized, resulting in poor chemical stability. It is difficult to guarantee long-term stability and cyclability, which restricts the application of lithium-sulfur solid electrolytes. Although Li 10 GeP2S 12 The lithium ion conductivity of (LGPS) can reach the level of commercial liquid electrolytes, but its cost is relatively high, and its application in sulfide solid electrolytes remains to be studied. The present invention replaces Ge with Bi to reduce the cost of the electrolyte, improve the lithium ion conductivity and the stability of lithium metal. Therefore, it is necessary to explore a solid electrolyte material with high ion conductivity and good chemical stability. Summary of the invention
[0004] The object of the present invention is to provide a bismuth-doped lithium germanium phosphorus sulfur solid electrolyte material and a preparation method thereof in view of the above defects or improvement requirements of the prior art. Specifically, it relates to a sulfide lithium ion solid electrolyte with high conductivity, that is, to provide a preparation method of a novel bismuth-doped lithium germanium phosphorus sulfur type solid electrolyte.
[0005] The object of the present invention is achieved by the following scheme:
[0006] The present invention provides a bismuth-doped lithium germanium phosphorus sulfur solid electrolyte material, and the chemical formula of the bismuth-doped lithium germanium phosphorus sulfur solid electrolyte material is Li x Ge 1-y Bi y P2S 12 , where 10 < x < 10.5, 0 < y < 0.5.
[0007] For the bismuth-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte, the range of x is preferably 10.05 ≤ x ≤ 10.2.
[0008] For the bismuth-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte, the range of y is preferably 0.05 ≤ y ≤ 0.2.
[0009] The present invention also provides a preparation method of a bismuth-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte, and the preparation method includes the following steps:
[0010] Step 1: According to the general formula: Li x Ge 1-y Bi y P2S 12 , where 10 < x < 10.5, 0 < y < 0.5, weigh Li2S, CeS2, Bi2S3, P2S5 in stoichiometric ratio;
[0011] Step 2: Grind and mix the raw materials of Li2S, CeS2, Bi2S3, P2S5 and then ball mill to obtain a mixed powder;
[0012] Step 3: Press the above mixed powder into tablets, put them into a sealed container, evacuate and then seal;
[0013] Step 4: Heat and calcine for solid-phase reaction;
[0014] Step 5: After the reaction is completed, naturally cool to room temperature to obtain a bismuth-doped lithium germanium phosphorus sulfur type solid electrolyte material with the composition of Li x Ge 1-y Bi y P2S 12 .
[0015] The bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte material replaces CeS2 with Bi2S3 at a certain stoichiometric ratio. Bi substitution produces a larger unit cell structure, making Li + The vacancies at the sites increase the diffusion of Li+ and the conductivity of the material. 2- Anion site disorder, Li + The sites will have vacancies and the optimal conductivity cannot be achieved. If the y value is too large, the raw material cost will increase, but the conductivity will change slightly.
[0016] Preferably, step 1, step 2 and step 3 are all carried out under an argon atmosphere. The water content of the argon is less than 1 ppm, and the oxygen content is less than 1 ppm.
[0017] Preferably, the ball milling speed in step 2 is 300-500 rpm, and the ball milling time is 5-30 hours.
[0018] Preferably, the pressing pressure in step 3 is 370-500 MPa, so that the components in the mixed raw materials are in closer contact and react more fully. The thickness of the flaky mixed powder is 1-15 mm.
[0019] Preferably, in step 4, the calcination temperature is 500-650°C, and the solid phase reaction time is 5-48 hours. If the reaction calcination temperature is too low, the reaction is incomplete; as the temperature increases, the grain size increases, which is conducive to the enhancement of densification. However, when the sintering temperature is too high, the irregular particles have a larger space due to the increase in size, which reduces the density. And when the temperature is too high, anisotropic thermal expansion causes material stress, causing voids and cracks in the material. As a result, the mobility of lithium ions is limited by larger grain boundaries, which is not conducive to obtaining higher conductivity.
[0020] The present invention also provides an application of the bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material in the preparation of an all-solid-state secondary battery.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The novel bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte material of the present invention has good chemical stability;
[0023] (2) Li obtained from the novel bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte of the present invention x Ge 1-y Bi y P2S 12 It has good ionic conductivity, reduces the activation barrier of lithium ion migration, and effectively solves the problem of Li x Ge 1-y Bi y P2S12 The lower ionic conductivity of sulfide solid electrolytes;
[0024] (3)Li x Ge 1-y Bi y P2S 12 Sulfide solid electrolytes improve the interfacial stability of lithium metal in lithium symmetric battery applications, show good cycle performance, and effectively solve the problem of Li 10 GeP2S 12 The problem of poor stability of sulfide solid electrolytes to lithium metal;
[0025] (4)Li x Ge 1-y Bi y P2S 12 Sulfide solid electrolyte has a simple preparation process and can be used as an ideal solid electrolyte material in all-solid-state lithium secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0027] Figure 1 The discharge-charge curve of the solid electrolyte material prepared in Example 1 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0028] Figure 2 The discharge-charge curve of the solid electrolyte material prepared in Example 2 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0029] Figure 3 The discharge-charge curve of the solid electrolyte material prepared in Example 3 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0030] Figure 4 The discharge-charge curve of the solid electrolyte material prepared in Example 4 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0031] Figure 5 The discharge-charge curve of the solid electrolyte material prepared in Comparative Example 1 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0032] Figure 6The discharge-charge curve of the solid electrolyte material prepared in Comparative Example 2 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C;
[0033] Figure 7 The discharge-charge curve of the solid electrolyte material prepared in comparative example 3 and the all-solid-state battery assembled with NCM811 as the positive electrode and LiIn as the negative electrode at a current density of 1C. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, which will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.
[0035] Example 1
[0036] A novel method for preparing a 5% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte is implemented, comprising the following steps:
[0037] Step 1: Grind and mix Li2S, CeS2, Bi2S3 and P2S5 in a molar ratio of 5.025:0.95:0.025:1 under an argon atmosphere to obtain a mixed powder. The mixed powder is sealed in a ball mill;
[0038] Step 2: Use a ball mill to grind the mixed powder. The speed of the ball mill is 400 rpm and the ball milling time is 24 hours;
[0039] Step 3, pressing the mixed powder into tablets, putting them into a sealed container, and packaging them after vacuuming;
[0040] Step 4, heating to 550°C and performing solid phase reaction for 8 hours;
[0041] Step 5: After the reaction is completed, naturally cool to room temperature to obtain a composition of Li 10.05 Ge 0.95 Bi 0.05 P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0042] Step 6, assemble into a sulfide solid-state battery: place 100 mg of the prepared bismuth-doped lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10 mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300 MPa. Finally, attach a LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 1 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 162 mAh.g -1 After 100 cycles of charge and discharge, the capacity remains at 135 mAh.g -1 ; The capacity retention rate of the full battery is about 83% after 100 cycles.
[0043] Example 2
[0044] A novel method for preparing a 10% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte is implemented, comprising the following steps:
[0045] Step 1: Grind and mix Li2S, CeS2, Bi2S3 and P2S5 in a molar ratio of 5.05:0.9:0.05:1 under an argon atmosphere to obtain a mixed powder. The mixed powder is sealed in a ball mill;
[0046] Step 2: Use a ball mill to grind the mixed powder. The speed of the ball mill is 400 rpm and the ball milling time is 24 hours;
[0047] Step 3, pressing the mixed powder into tablets, putting them into a sealed container, and packaging them after vacuuming;
[0048] Step 4, heating to 550°C and performing solid phase reaction for 8 hours;
[0049] Step 5: After the reaction is completed, naturally cool to room temperature to obtain a composition of Li 10.1 Ge 0.9 Bi 0.1 P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0050] Step 6, assemble into a sulfide solid-state battery: place 100 mg of the prepared bismuth-doped lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10 mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300 MPa. Finally, attach a LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 2 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 170 mAh.g-1 After 100 cycles of charge and discharge, the capacity remains at 142 mAh.g -1 ; The capacity retention rate of the full battery is about 84% after 100 cycles.
[0051] Example 3
[0052] A novel method for preparing a 15% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte is implemented, comprising the following steps:
[0053] Step 1: Grind and mix Li2S, CeS2, Bi2S3 and P2S5 in a molar ratio of 5.075:0.85:0.075:1 under an argon atmosphere to obtain a mixed powder. The mixed powder is sealed in a ball mill;
[0054] Step 2: Use a ball mill to grind the mixed powder. The speed of the ball mill is 400 rpm and the ball milling time is 24 hours;
[0055] Step 3, pressing the mixed powder into tablets, putting them into a sealed container, and packaging them after vacuuming;
[0056] Step 4, heating to 550°C and performing solid phase reaction for 8 hours;
[0057] Step 5: After the reaction is completed, naturally cool to room temperature to obtain a composition of Li 10.15 Ge 0.85 Bi 0.15 P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0058] Step 6, assemble into a sulfide solid-state battery: place 100 mg of the prepared bismuth-doped lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10 mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300 MPa. Finally, attach a LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 3 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 187 mAh.g -1 After 100 cycles of charge and discharge, the capacity remains at 165 mAh.g -1 ; The capacity retention rate of the full battery is about 88% after 100 cycles.
[0059] Example 4
[0060] A novel method for preparing a 20% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte is implemented, comprising the following steps:
[0061] Step 1: Grind and mix Li2S, CeS2, Bi2S3 and P2S5 in a molar ratio of 5.1:0.8:0.1:1 under an argon atmosphere to obtain a mixed powder. The mixed powder is sealed in a ball mill;
[0062] Step 2: Use a ball mill to grind the mixed powder. The speed of the ball mill is 400 rpm and the ball milling time is 24 hours;
[0063] Step 3, pressing the mixed powder into tablets, putting them into a sealed container, and packaging them after vacuuming;
[0064] Step 4, heating to 550°C and performing solid phase reaction for 8 hours;
[0065] Step 5: After the reaction is completed, naturally cool to room temperature to obtain a composition of Li 10.2 Ge 0.8 Bi 0.2 P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0066] Step 6, assemble into a sulfide solid-state battery: place 100 mg of the prepared bismuth-doped lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10 mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300 MPa. Finally, attach a LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 4 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 167 mAh.g -1 After 100 cycles of charge and discharge, the capacity remains at 145 mAh.g -1 ; The capacity retention rate of the full battery is about 87% after 100 cycles.
[0067] Comparative Example 1
[0068] The comparative example is a novel 30% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte, and the preparation method is basically the same as that of Example 1, except that Li2S, CeS2, Bi2S3, and P2S5 are mixed in a molar ratio of 5.15:0.7:0.15:1 to obtain a composition of Li 10.3 Ge 0.7 Bi 0.3 P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0069] Assemble into sulfide solid-state battery: Place 100mg of the prepared bismuth-doped lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300Mpa. Finally, attach a LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 5 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 155 mAh.g -1 After 100 cycles of charge and discharge, the capacity remains at 124 mAh.g -1 ; The capacity retention rate of the full battery is about 80% after 100 cycles.
[0070] Comparative Example 2
[0071] The comparative example is a lithium germanium phosphorus sulfur type solid electrolyte without bismuth. The preparation method is basically the same as that of Example 1, except that Li2S, CeS2 and P2S5 are mixed in a molar ratio of 5:1:1 to obtain a Li 10 GeP2S 12 Bismuth-free lithium-germanium-phosphorus-sulfur solid electrolyte material.
[0072] Assemble into sulfide solid-state battery: Place 100mg of lithium germanium phosphorus sulfur sulfide solid electrolyte powder in a tablet pressing mold and press it into a solid electrolyte sheet. Then place 10mg of NCM811 positive electrode sheet on one side of the solid electrolyte and press it at 300Mpa. Finally, attach LiIn sheet on the other side of the solid electrolyte and press it into a full solid-state battery. Test the cycle stability of the obtained sulfide solid-state battery at room temperature. Figure 6 It can be seen that the initial specific capacity of the assembled full battery at 1C rate is 149 mAh.g -1 After 100 cycles of charge and discharge, the capacity remains at 102 mAh.g -1 ; The capacity retention rate of the full battery is about 70% after 100 cycles.
[0073] Comparative Example 3
[0074] The comparative example is a novel 5% bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte, and the preparation method is basically the same as that of Example 1, except that the calcination temperature is 300°C.
[0075] like Figure 7 As shown, the initial specific capacity of the assembled full battery is 83 mAh.g at 1C rate. -1 After 10 cycles of charge and discharge, the capacity is only 64 mAh.g -1 .
[0076] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A method for preparing a bismuth-doped lithium germanium phosphorus-sulfur solid electrolyte material, characterized in that: The general chemical formula is: Li x Ge 1-y Bi y P2S 12 , wherein 10.05≤x≤10.2, 0.05≤y≤0.2; the preparation method comprises the following steps: Step 1, according to the general formula: Li x Ge 1-y Bi y P2S 12 , weigh Li2S, CeS2, Bi2S3, P2S5 in stoichiometric ratio; Step 2, grinding and mixing Li2S, CeS2, Bi2S3, and P2S5 raw materials and then ball milling to obtain a mixed powder; Step 3, pressing the mixed powder into tablets, putting them into a sealed container, and packaging them after vacuuming; Step 4, heating and calcining to carry out solid phase reaction; Step 5: After the reaction is completed, naturally cool to room temperature to obtain a composition of Li x Ge 1-y Bi y P2S 12 Bismuth-doped lithium-germanium-phosphorus-sulfur solid electrolyte material.
2. The preparation method according to claim 1, characterized in that: Step 1, step 2 and step 3 are all carried out under an argon atmosphere.
3. The preparation method according to claim 1, characterized in that: The ball milling speed in step 2 is 300 to 500 rpm, and the ball milling time is 5 to 30 hours.
4. The preparation method according to claim 1, characterized in that: The pressing pressure in step 3 is 370-500 MPa.
5. The preparation method according to claim 1, characterized in that: The thickness of the flaky mixed powder is 1 to 15 mm.
6. The preparation method according to claim 1, characterized in that: In step 4, the calcination temperature is 500-650° C., and the solid phase reaction time is 5-48 hours.
7. Use of the lithium germanium phosphorus sulfur type solid electrolyte material obtained by the preparation method as claimed in claim 1 in the preparation of an all-solid-state secondary battery.
Citation Information
Patent Citations
Composite electrolyte, lithium metal battery comprising same, and method of preparing composite electrolyte
CN111048828A
Lithium-containing argyrodite solid electrolyte with dopant and preparation method of lithium-containing argyrodite solid electrolyte
CN111430808A
Separable and recyclable sulfide type solid electrolyte and application thereof
CN111834664A
Halide solid electrolyte, preparation method and application thereof, and all-solid-state lithium ion battery
CN113097559A
Sulfide solid electrolyte
JP2019125502A
Cited By
Preparation method of lithium-germanium-phosphorus-sulfur solid-state battery
CN120341400A