A PVDF composite energy storage material and preparation method thereof
By filling TiO2 nanosheets and nanowires in PVDF, the energy storage density and dielectric constant are increased, which solves the problem of insufficient density of existing energy storage materials and achieves efficient energy storage material preparation and cost reduction.
Patent Information
- Application Number
- CN202210545142.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-05-19
AI Technical Summary
The low dielectric constant of existing energy storage materials results in insufficient energy storage density, which limits their use in fast charging and discharging applications, and the process is complex and costly.
Polyvinylidene fluoride (PVDF) is filled with TiO2 nanosheets and TiO2 nanowires. The breakdown strength and dielectric constant of the composite material are improved through trace filling. The volume ratio and dimensional regular configuration are used to increase the energy storage density.
It has achieved a significant increase in energy storage density, reaching a maximum of 17.6J/cm3, simplified the material preparation process, reduced costs, and is suitable for industrial production.
Smart Images

Figure CN114927345B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an energy storage material and a preparation method thereof, and in particular to a PVDF composite energy storage material and a preparation method thereof. Background Art
[0002] At present, countries around the world are generally facing the problem of energy depletion, and have put forward high requirements for the development of new energy. Clean and renewable energy such as solar energy, wind energy and geothermal energy are usually intermittent and uncontrollable, so they need to be collected, stored and converted. Dielectric energy storage capacitors can release stored energy in a very short time and generate high-power pulses. They have broad application prospects in pulse power systems, especially in hybrid vehicles and grid-connected photovoltaic power generation.
[0003] High energy storage density materials have an important impact on the development of electronic power systems, especially in applications that require fast charging and discharging. Common energy storage density materials are mainly oxide ceramics and polymer dielectric materials. Oxide ceramics are widely used as energy storage materials due to their high dielectric constant and stable performance, but their application is limited by expensive raw materials and complex processes. Compared with oxide ceramics, although polymer dielectric materials have good flexibility, lower manufacturing temperature and cost, their low energy storage density due to the low dielectric constant limits their application. Summary of the invention
[0004] Purpose of the invention: The first purpose of the present invention is to provide a PVDF composite energy storage material with improved energy storage density; the second purpose of the present invention is to provide a method for preparing the energy storage material.
[0005] Technical solution: The energy storage material described in the present invention is composed of TiO2 filled in polyvinylidene fluoride, wherein the TiO2 content is 2vol% to 10vol%, and the rest is polyvinylidene fluoride (PVDF); the TiO2 is composed of TiO2 nanosheets and TiO2 nanowires in a volume ratio of 4 to 6:1.
[0006] The composite energy storage material improves the breakdown strength of the composite material by filling a small amount of TiO2 nanosheets, improves the dielectric constant and electric displacement of the composite material as a whole by filling a small amount of TiO2 nanowires, and finally improves the energy storage density of the composite material by the regular configuration of the dimensions of the filler. The volume ratio of the TiO2 nanosheets and the TiO2 nanowires, as well as the overall volume fraction in the composite energy storage material, affect the energy storage density of the energy storage material.
[0007] TiO2 nanosheets and nanowires refer to sheet-like or linear structures with at least one dimension in nanometer size in three-dimensional space.
[0008] Preferably, the length and width of the TiO2 nanosheet are both 300nm to 400nm, and the thickness is 3nm to 5nm.
[0009] Preferably, the diameter of the TiO2 nanowire is 20nm-100nm, and the length is 5-10μm.
[0010] The method for preparing the energy storage material of the present invention comprises the following steps:
[0011] (1) Preparation of TiO2 nanowires
[0012] The titanium dioxide powder is added to a sodium hydroxide aqueous solution to prepare a suspension, and then hydrothermally reacted at 160-200° C. for 40-50 hours; a white precipitate is obtained by cooling, washed to neutrality, and calcined at 560-600° C. for 1-3 hours to obtain TiO2 nanowires;
[0013] (2) Preparation of TiO2 nanosheets
[0014] Tetrabutyl titanate, 48% hydrofluoric acid by mass and ethanol are mixed and subjected to hydrothermal reaction at 180-190° C. for 10-14 hours; powder precipitates are recovered, washed and dried to obtain TiO2 nanosheets;
[0015] (3) Preparation of energy storage materials
[0016] The TiO2 nanowires, TiO2 nanosheets and PVDF are uniformly mixed, pressed into sheets, and finally sintered at 160-200°C for 30-40 minutes to obtain a composite energy storage material.
[0017] In the step (2), the role of tetrabutyl titanate is to provide titanium element, the role of hydrofluoric acid is to modify the surface of TiO2, expose the {001} surface, and form a sheet structure. Ethanol is another surface modifier, which enhances the exposure of the {001} surface and finally forms a nanosheet.
[0018] In the step (3), heat treatment to form a dense composite material is a step in preparing the material and has a great impact on the performance. Too high a temperature or too long a time may cause PVDF to decompose and affect the final performance.
[0019] Preferably, in step (1), the concentration of the sodium hydroxide aqueous solution is 10 to 12 mol / L; the temperature of the hydrothermal reaction is 180 to 200° C., and the reaction time is 45 to 50 hours; the calcination temperature is 580 to 600° C., and the time is 2 to 3 hours.
[0020] Preferably, in step (2), the volume ratio of tetrabutyl titanate, hydrofluoric acid and ethanol is 10-20:4.5-9:5-10.
[0021] Preferably, in step (2), the drying temperature is 80° C. and the drying time is 1 to 3 hours.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The composite energy storage material uses a small amount of TiO2 nanosheets to improve the breakdown strength of the composite material, and uses a small amount of TiO2 nanowires to improve the overall dielectric constant and electric displacement of the composite material. Finally, the energy storage density of the composite material is improved by the regular configuration of the dimensions of the filler, and the energy storage density can reach up to 17.6 J / cm 3 (2) The preparation method has low material cost, simple process and is easy for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the PVDF composite energy storage material of the present invention;
[0024] Figure 2 This is a surface scanning electron microscope image of the composite energy storage material prepared in Example 1;
[0025] Figure 3 A scanning electron microscope image of TiO2 nanowires prepared in Example 2;
[0026] Figure 4 An atomic force microscope image of the TiO2 nanosheet prepared in Example 2;
[0027] Figure 5 A transmission electron microscopy image of the TiO2 nanosheets prepared in Example 2;
[0028] Figure 6 The Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Example 1;
[0029] Figure 7 The electric displacement curve of the composite energy storage material prepared in Example 1;
[0030] Figure 8 The energy storage density diagram of the composite energy storage material prepared in Example 1;
[0031] Fig. 9 The frequency curve of the dielectric constant of the composite energy storage material prepared in Example 1;
[0032] Fig.10 The Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Example 2;
[0033] Fig.11 The electric displacement curve of the composite energy storage material prepared in Example 2;
[0034] Fig.12 The energy storage density diagram of the composite energy storage material prepared in Example 2;
[0035] Fig.13The frequency curve of the dielectric constant of the composite energy storage material prepared in Example 2;
[0036] Fig.14 The Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Example 3;
[0037] Fig.15 The electric displacement curve of the composite energy storage material prepared in Example 3;
[0038] Fig.16 This is the energy storage density diagram of the composite energy storage material prepared in Example 3;
[0039] Fig.17 The frequency curve of the dielectric constant of the composite energy storage material prepared in Example 3;
[0040] Fig.18 Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Comparative Example 1;
[0041] Fig.19 The electric displacement curve of the composite energy storage material prepared in Comparative Example 1;
[0042] Fig. 20 This is the energy storage density diagram of the composite energy storage material prepared in Comparative Example 1;
[0043] Fig.21 The frequency curve of the dielectric constant of the composite energy storage material prepared in Comparative Example 1;
[0044] Fig. 22 Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Comparative Example 2;
[0045] Fig.23 The electric displacement curve of the composite energy storage material prepared in Comparative Example 2;
[0046] Fig.24 This is the energy storage density diagram of the composite energy storage material prepared in Comparative Example 2;
[0047] Fig.25 The frequency curve of the dielectric constant of the composite energy storage material prepared in Comparative Example 2;
[0048] Fig.26 Weibull distribution diagram of the breakdown strength of the composite energy storage material prepared in Comparative Example 3;
[0049] Fig. 27 The electric displacement curve of the composite energy storage material prepared in Comparative Example 3;
[0050] Fig.28 This is the energy storage density diagram of the composite energy storage material prepared in Comparative Example 3;
[0051] Fig.29The frequency curve of the dielectric constant of the composite energy storage material prepared in Comparative Example 3;
[0052] Fig.30 The figure is a bar chart comparing the data of Examples 1-3 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below in conjunction with embodiments.
[0054] Example 1
[0055] The PVDF composite energy storage material of the present invention has a TiO2 content of 2 vol% and the rest is polyvinylidene fluoride, wherein the TiO2 is composed of TiO2 nanosheets and TiO2 nanowires in a volume ratio of 4:1; and the preparation method thereof comprises the following steps:
[0056] (1) Preparation of TiO2 nanowires
[0057] In a 50mL beaker, 1g of titanium dioxide powder was added to 20mL of sodium hydroxide solution (10mol / L) and stirred for 10 minutes; the obtained suspension was transferred to a cylindrical autoclave lined with polytetrafluoroethylene and hydrothermally reacted at 160°C for 40h; a white precipitate was obtained after cooling and recovery, which was washed with 0.1mol / L HCl solution, neutralized with deionized water to a pH value of 7-8, and then repeatedly rinsed with deionized water, and the particles were recovered by vacuum filtration, and TiO2 nanowires were obtained after calcination at 560°C for 1h.
[0058] (2) Preparation of TiO2 nanosheets
[0059] Add 10 mL of tetrabutyl titanate, 4.5 mL of hydrofluoric acid (mass fraction 48%) and 5 mL of ethanol into a reaction container and stir. Transfer the resulting solution into a cylindrical autoclave lined with polytetrafluoroethylene and keep it at 180°C for 10 hours. Recover the particles by vacuum filtration, wash with deionized water, and then dry at 80°C for 1 hour to obtain TiO2 nanosheets.
[0060] (3) Preparation of energy storage materials
[0061] TiO2 nanosheets and TiO2 nanowires were mixed with PVDF in a volume ratio of 4:1, with the TiO2 nanosheets and TiO2 nanowires accounting for 2% of the total volume. After being stirred evenly, the mixture was placed into a tablet pressing mold for tablet pressing, and finally sintered at 180°C for 30 minutes to obtain a composite energy storage material.
[0062] Example 2
[0063] The PVDF composite energy storage material of the present invention has a TiO2 content of 8 vol% and the rest is polyvinylidene fluoride, wherein the TiO2 is composed of TiO2 nanosheets and TiO2 nanowires in a volume ratio of 5:1; and the preparation method thereof comprises the following steps:
[0064] (1) Preparation of TiO2 nanowires
[0065] In a 50mL beaker, add 1.5g of titanium dioxide powder to 20mL of sodium hydroxide solution (11mol / L) and stir for 10 minutes. The obtained suspension was transferred to a cylindrical autoclave lined with polytetrafluoroethylene and subjected to hydrothermal treatment at 180°C for 45h. After cooling and recovery, a white precipitate was obtained, which was washed with 0.1mol / L HCl solution, neutralized with deionized water to a pH of 7-8, and then repeatedly rinsed with deionized water. The particles were recovered by vacuum filtration and calcined at 580°C for 2h to obtain TiO2 nanowires with a diameter of 20nm-100nm and a length of 5-10μm (such as Figure 3 shown).
[0066] (2) Preparation of TiO2 nanosheets
[0067] 15 mL of tetrabutyl titanate, 6.75 mL of hydrofluoric acid (mass fraction 48%) and 7.5 mL of ethanol were added to the reaction vessel and stirred. The resulting solution was transferred to a cylindrical autoclave lined with polytetrafluoroethylene and kept at 180°C for 12 hours. The resulting solution was vacuum filtered to recover particles, then washed with deionized water and dried at 80°C for 2 hours to obtain TiO2 nanosheets with a length and width of 300 nm to 100 nm and a thickness of 1.30 mm to 1.40 mm (e.g. Figure 4 and 5 shown).
[0068] (3) Preparation of energy storage materials
[0069] TiO2 nanosheets and TiO2 nanowires were mixed with PVDF in a volume ratio of 5:1, with the TiO2 nanosheets and TiO2 nanowires accounting for 8% of the total volume. After being stirred evenly, the mixture was put into a tablet pressing mold for tablet pressing, and finally sintered at 180°C for 40 minutes to obtain a composite energy storage material.
[0070] Example 3
[0071] The PVDF composite energy storage material of the present invention has a TiO2 content of 10 vol% and the rest is polyvinylidene fluoride, wherein the TiO2 is composed of TiO2 nanosheets and TiO2 nanowires in a volume ratio of 6:1; and the preparation method thereof comprises the following steps:
[0072] (1) Preparation of TiO2 nanowires
[0073] In a 50mL beaker, add 2g of titanium dioxide powder to 25mL of sodium hydroxide solution (12mol / L) and stir for 10 minutes. Transfer the obtained suspension to a cylindrical autoclave lined with polytetrafluoroethylene and perform hydrothermal treatment at 200℃ for 50h. After cooling and recovery, a white precipitate is obtained, which is washed with 0.1mol / L HCl solution, neutralized with deionized water to a pH value of 7-8, and then repeatedly rinsed with deionized water, and the particles are recovered by vacuum filtration. TiO2 nanowires are obtained after calcination at 600℃ for 3h.
[0074] (2) Preparation of TiO2 nanosheets
[0075] 20 mL of tetrabutyl titanate, 9 mL of hydrofluoric acid (mass fraction 48%) and 10 mL of ethanol were added to the reaction vessel, stirred, and the obtained solution was transferred to a cylindrical autoclave lined with polytetrafluoroethylene and kept at 180°C for 14 hours. The obtained solution was vacuum filtered to recover particles, then washed with deionized water, and then dried at 80°C for 3 hours to obtain TiO2 nanosheets.
[0076] (3) Preparation of energy storage materials
[0077] TiO2 nanosheets and TiO2 nanowires were mixed with PVDF in a volume ratio of 6:1, with the volume fraction of the composite material being 10%. After being stirred evenly, the mixture was put into a tablet pressing mold for tablet pressing, and finally sintered at 200°C for 30 minutes to obtain a composite energy storage material.
[0078] Comparative Example 1
[0079] On the basis of Example 2, TiO2 nanowires and TiO2 nanosheets are not added, PVDF is used to synthesize the energy storage material, and other conditions remain unchanged.
[0080] Comparative Example 2
[0081] On the basis of Example 2, TiO2 nanowires are not added, and TiO2 nanosheets accounting for 8% of the total volume are used to synthesize the energy storage material with PVDF, while other conditions remain unchanged.
[0082] Comparative Example 3
[0083] On the basis of Example 2, no TiO2 nanosheets were added, and TiO2 nanowires accounting for 8% of the total volume were used to synthesize the energy storage material with PVDF, while other conditions remained unchanged.
[0084] Performance Testing
[0085] The breakdown strength, electric displacement, energy storage density and dielectric constant of the energy storage materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested. The breakdown strength test was performed using a Changsheng Cs2674ax ultra-high voltage tester; the electric displacement test was performed using an aixACCT TFanalyzer 2000 ferroelectric tester; the dielectric constant test was performed using an LCR digital bridge; the energy storage density diagram was obtained by testing with a ferroelectric tester, and the energy storage density was calculated according to the formula U=∫EdD. The test results are shown in Table 1.
[0086] Table 1 Test results of dielectric constant and energy storage density of energy storage materials
[0087]
[0088] Among Examples 1 to 3, the energy storage density of the product prepared according to the formula used in Example 2 is the highest, which is 17.6 J / cm 3 As the TiO2 loading increases, the energy storage performance also increases. This is because TiO2 nanosheets and nanowires can respectively improve the breakdown strength and electrical displacement of the composite material, ultimately achieving an increase in energy storage density. However, at higher loadings, organic / inorganic interface defects will also increase, resulting in a decrease in performance.
[0089] The breakdown strength, electric displacement, energy storage density and dielectric constant of the energy storage materials of Comparative Examples 1 to 3 all show different degrees of decrease compared with Example 2, which indicates that the performance of a single material filled with TiO2 nanowires or nanosheets is not as good as that filled with both nanowires and nanosheets at the same time without filling with TiO2 nanosheets and nanowires. This is because TiO2 nanosheets and nanowires can respectively improve the breakdown strength and electric displacement of the composite material, and ultimately achieve an increase in energy storage density.
Claims
1. A PVDF composite energy storage material, It is characterized in that Filling TiO in PVDF 2 , where TiO 2 The content is 2 vol% to 10 vol%, and the rest is polyvinylidene fluoride; the TiO 2 TiO 2 Nanosheets and TiO 2 The nanowires are composed of a volume ratio of 4 to 6:1; the TiO 2 The diameter of the nanowire is 20 nm to 100 nm, and the length is 5 to 10 μm; the length and width of the TiO2 nanosheet are both 300 nm to 400 nm, and the thickness is 3 nm to 5 nm.
2. A method for preparing the energy storage material according to claim 1, It is characterized in that The following steps are involved: (1) Preparation of TiO 2 Nanowires Titanium dioxide powder is added to a sodium hydroxide aqueous solution to prepare a suspension, and then hydrothermally reacted at 160-200°C for 40-50 hours; cooled to obtain a white precipitate, washed to neutrality, and calcined at 560-600°C for 1-3 hours to obtain TiO 2 Nanowires; (2) Preparation of TiO 2 Nanosheets Tetrabutyl titanate, hydrofluoric acid and ethanol are mixed and subjected to hydrothermal reaction at 180-190°C for 10-14 hours; the powder precipitate is recovered, washed and dried to obtain TiO 2 Nanosheets; (3) Preparation of energy storage materials TiO 2 Nanowires, TiO 2 The nanosheets and PVDF are mixed evenly, pressed into sheets, and finally sintered at 160-200° C. for 30-40 minutes to obtain a composite energy storage material.
3. The method for preparing the energy storage material according to claim 2, It is characterized in that In step (1), the concentration of the sodium hydroxide aqueous solution is 10-12 mol / L.
4. The method for preparing the energy storage material according to claim 2, It is characterized in that In step (2), the tetrabutyl titanate, hydrofluoric acid and ethanol are in a volume ratio of 10-20:4.5-9:5-10.
5. The method for preparing the energy storage material according to claim 2, It is characterized in that In step (1), the temperature of the hydrothermal reaction is 180-200° C. and the time is 45-50 hours.
6. The method for preparing the energy storage material according to claim 2, It is characterized in that In step (1), the calcination temperature is 580-600° C. and the calcination time is 2-3 hours.
Citation Information
Patent Citations
Built-in high-dielectric-constant flexible resin composite material, and preparation method and application thereof
CN107573645A