A low-temperature curing conductive silver paste for HJT high-efficiency batteries and a preparation method thereof

By using low-temperature curing conductive silver paste in HJT batteries, combined with the optimized ratio of silver-coated copper powder, dendritic silver powder and organic carrier and Re2O7 inhibitor, the problem of damage to the passivation layer of HJT batteries caused by existing conductive silver paste is solved. It achieves efficient photoelectric conversion and high conductivity suitable for industrial production.

CN114937518BActive Publication Date: 2024-10-29DK ELECTRONICS MATERIALS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210641600.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-07
Publication Date
2024-10-29
Estimated Expiration
2042-06-07

AI Technical Summary

Technical Problem

Existing conductive silver paste is not suitable for HJT high-efficiency cells, resulting in damage to the passivation layer and reduced photoelectric conversion efficiency, and cannot meet the high-efficiency production needs of HJT cells.

Method used

Develop a low-temperature curing conductive silver paste containing 60-72 parts of silver-coated copper powder, 12-24 parts of dendritic silver powder, 8-13 parts of coupling agent, 38-45 parts of organic carrier and 3-6 parts of inhibitors. Value particle size and viscosity are optimized, using a combination of epoxy resin and coupling agent, adding Re2O7 inhibitor to prevent excessive sintering and form excellent ohmic contact.

Benefits of technology

The low-temperature curing conductive silver paste achieves high conductivity and excellent photoelectric conversion efficiency in HJT cells, which is suitable for large-scale industrial production and significantly improves the conversion efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114937518B_ABST
    Figure CN114937518B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of HJT high-efficiency battery materials, and specifically relates to a low-temperature curing conductive silver paste for HJT high-efficiency batteries and a preparation method thereof. In parts by mass, the low-temperature curing conductive silver paste comprises the following components: 60-72 parts of silver-coated copper powder, 12-24 parts of dendritic silver powder, 8-13 parts of coupling agent, 38-45 parts of organic carrier, and 3-6 parts of inhibitor. When the low-temperature curing conductive silver paste is used as a slurry for HJT high-efficiency batteries, it can produce excellent ohmic contact performance, showing high conductivity and excellent photoelectric conversion efficiency, and is therefore particularly suitable for large-scale industrial production of HJT solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of HJT high-efficiency battery materials, and specifically relates to a low-temperature curing conductive silver paste for HJT high-efficiency batteries and a preparation method thereof. Background Art

[0002] At present, the mainstream solar cell products in the market are P-type monocrystalline PERC cells. However, the efficiency of P-type PERC cells has reached its upper limit. With the expansion of market demand and the continuous development of industry technology, N-type crystalline silicon solar cell technology has received more and more attention in recent years, which mainly includes passivated emitter back surface fully diffused cells (n-PERT), tunnel oxide passivated contact cells (TOPCon) and heterojunction cells (HJT). N-type crystalline silicon solar cells have further improved the conversion efficiency of crystalline silicon solar cells.

[0003] HJT cells use low-cost amorphous silicon as the emission layer, and its emission layer is doped amorphous silicon material. When depositing single-crystalline silicon, only about 200°C is needed to meet the preparation temperature requirements. The low-temperature process also ensures that the interface damage of the single-crystalline silicon substrate is lower, and the presence of the intrinsic layer makes the interface passivation performance better.

[0004] The conductive silver paste used in the current mainstream P-type photovoltaic cells in the market is not suitable for preparing electrodes for HJT cells. The conductive silver paste used in P-type photovoltaic cells will burn through the passivation layer structure, resulting in a loss in the fill factor (FF) and open circuit voltage (Uoc) of the cell, seriously affecting the photoelectric conversion efficiency of the solar cell.

[0005] Therefore, a new type of conductive silver paste is developed to reduce the damage to the passivation layer of HJT high-efficiency batteries during the battery sintering process. It is more suitable for solar cells with transparent conductive film structures (such as indium antimony oxide structures), so that they can achieve higher photoelectric conversion efficiency, which plays a very important role in the development of future high-efficiency batteries.

[0006] Therefore, it is urgent to develop a new low-temperature conductive slurry that is suitable for large-scale industrial production of HJT high-efficiency batteries. Summary of the invention

[0007] In view of the technical defects existing in the prior art, the technical solution provided by the present invention aims to provide a new conductive silver paste, which, when used as a conductive paste for HJT solar cells, can produce excellent ohmic contact performance, exhibit high conductivity and excellent photoelectric conversion efficiency, and thus has broad application prospects.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] The first aspect of the present invention provides a low-temperature curing conductive silver paste for HJT high-efficiency batteries, which comprises the following components, in parts by mass: 60-72 parts of silver-coated copper powder, 12-24 parts of dendritic silver powder, 8-13 parts of coupling agent, 38-45 parts of organic carrier, and 3-6 parts of inhibitor;

[0010] Wherein, the organic carrier is composed of an adhesive resin and an organic solvent;

[0011] Wherein, the median particle size of the silver-coated copper powder is 55-90nm;

[0012] The median particle size of the dendritic silver powder is 3-6 μm.

[0013] It is worth noting that the silver-coated copper powder or the dendritic silver powder is an existing product available on the market, or a product that can be prepared according to the technical solution described in the prior art, so it is not described in detail herein. In addition, the silver-coated copper powder can be in the form of flakes or spheres. The silver-coated copper powder and the dendritic silver powder are used in combination to increase the effective specific surface area of ​​Ag.

[0014] In particular, the use of silver-coated copper powder effectively reduces the use of expensive silver powder, so the production cost of the electronic paste is significantly reduced; in addition, the resistance and density of silver-coated copper powder are between silver powder and copper powder, and the resistance decreases with the increase of pressure, while the specific surface area of ​​silver-coated copper powder is higher than that of silver powder and copper powder. Silver-coated copper is prone to oxidation failure in the traditional PERC high-temperature process, and the low-temperature process of HJT can inhibit the oxidation of copper, so silver-coated copper has great potential to be promoted and applied in HJT.

[0015] The organic carrier helps to mechanically mix and evenly disperse the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor, so that the low-temperature curing conductive silver paste has suitable viscosity and rheological properties.

[0016] Preferably, in the above-mentioned low-temperature curing conductive silver paste, the coupling agent is selected from any one or more combinations of the following: isopropyl trioleyl titanate, isopropyl triisostearyl titanate, isopropyl tri(isooctanoyl) titanate, isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl di(methacryloyl) isostearyl titanate, isopropyl tri(isostearoyl) titanate, and isopropyl tri(dioctyl pyrophosphoryl) titanate.

[0017] Additionally preferably, the low-temperature curing conductive silver paste described in the first aspect may also contain other additives. The other additives are one or more of a leveling agent, a thickener and a thixotropic agent. Specifically, the leveling agent is preferably: an acrylic leveling agent, such as a pure acrylic leveling agent, a modified acrylic leveling agent; an organosilicon leveling agent, such as polymethyl alkyl siloxane, an organic modified polysiloxane; a fluorocarbon leveling agent. The thickener is preferably one or more of sodium fatty acid and tricalcium phosphate. The thixotropic agent is preferably hydrogenated castor oil and / or gum, which can improve the thixotropy of the conductive silver paste, so that the conductive silver paste has a higher consistency when stationary, and can become a low-viscosity fluid under the action of external force.

[0018] Preferably, in the above-mentioned low-temperature curing conductive silver paste, the mass ratio of the adhesive resin to the organic solvent is 1:5 to 1:8. On this basis, further preferably, the mass ratio of the adhesive resin to the organic solvent is 1:5 to 1:7; further preferably, the mass ratio of the adhesive resin to the organic solvent is 1:6.

[0019] Preferably, in the above-mentioned low-temperature curing conductive silver paste, the adhesive resin is selected from any one or more combinations of the following: epoxy resin, acrylic resin, phenolic resin, and melamine urea-formaldehyde resin.

[0020] Further preferably, in the above-mentioned low-temperature curing conductive silver paste, the adhesive resin is epoxy resin.

[0021] Further preferably, in the above-mentioned low-temperature curing conductive silver paste, the adhesive resin is melamine urea-formaldehyde resin.

[0022] Further preferably, in the above-mentioned low-temperature curing conductive silver paste, the adhesive resin is a phenolic resin.

[0023] In addition, during the research and development process, the inventors unexpectedly discovered that when epoxy resin is selected as the adhesive resin and used in combination with the above-mentioned coupling agent, the above-mentioned low-temperature curing conductive silver paste can obtain a sufficiently low resistivity (≤4×10-6Ω·cm) and exhibit an ideal extremely low viscosity (60~120Pa.s).

[0024] Specifically, when the adhesive resin is an epoxy resin, the coupling agent is preferably isopropyl triisostearate titanate; the coupling agent may also be preferably isopropyl dioleyloxy (dioctylphosphoyloxy) titanate; the coupling agent may also be preferably isopropyl di(methacryloyl) isostearyl titanate; the coupling agent may also be preferably isopropyl tri(isostearyl) titanate; the coupling agent may also be preferably isopropyl tri(dioctyl pyrophosphoyl) titanate.

[0025] When the adhesive resin is an epoxy resin, the coupling agent is further preferably a combination of isopropyl tri(isostearoyl) titanate and isopropyl tri(dioctyl pyrophosphoryl) titanate; in this case, the viscosity of the low-temperature curing conductive silver paste is 80~100 Pa.s.

[0026] On this basis, the mass ratio of the isopropyl tri(isostearoyl) titanate to the isopropyl tri(dioctyl pyrophosphoryl) titanate is 1:1.

[0027] Exemplarily, the epoxy resin can be a combination of any one or more of the following: 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, hexahydrophthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, 1,2-epoxy-4-vinylcyclohexane, vinylcyclohexene-diepoxide, bisphenol A epoxy resin, aliphatic epoxy resin, bisphenol F epoxy resin or bisphenol S epoxy resin.

[0028] Preferably, in the above-mentioned low-temperature curing conductive silver paste, the organic solvent is selected from any one or more combinations of the following: terpineol, dihydroterpineol, ethylene glycol phenyl ether, propylene glycol phenyl ether, butyl carbitol, butyl carbitol acetate, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, dihydroterpineol acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0029] Further preferably, in the above-mentioned low-temperature curing conductive silver paste, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether. On this basis, further preferably, the volume ratio of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether is 1:2:1; further preferably, the volume ratio of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether is 1:1:1; further preferably, the volume ratio of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether is 2:1:1; further preferably, the volume ratio of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether is 1:1:2; most preferably, the volume ratio of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether is 2:1:2.

[0030] Preferably, in the above-mentioned low temperature curing conductive silver paste, the inhibitor is Re 2 O 7 . 2 O 7 The addition of can prevent excessive sintering of silver-coated copper powder and dendritic silver powder, which is conducive to forming excellent ohmic contact, thereby significantly improving the photoelectric conversion efficiency.

[0031] In addition, the second aspect of the present invention provides a method for preparing the low-temperature curing conductive silver paste according to the first aspect, comprising the following steps:

[0032] S1: weighing an adhesive resin and an organic solvent according to a certain mass ratio, adding the adhesive resin into the organic solvent, heating and stirring to obtain an organic carrier;

[0033] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0034] S3: subjecting the coarse mixed slurry to vacuum degassing treatment; and

[0035] S4: grinding to obtain the low-temperature curing conductive silver paste.

[0036] Preferably, in the above preparation method, in S1, the heating temperature is 160-190° C., and the heating duration is 15-35 minutes.

[0037] Preferably, in the above preparation method, in S3, the vacuum degree of the vacuum degassing treatment is 0.08-0.12 MPa, and the duration of the vacuum degassing treatment is 12-20 minutes.

[0038] In addition, in the above preparation method, operations such as stirring and grinding are conventional operations known to those skilled in the art, and therefore will not be described in detail herein.

[0039] The third aspect of the present invention also provides the use of the low temperature curing conductive silver paste described in the first aspect in HJT high efficiency cells. Specifically, the electrode containing the low temperature curing conductive silver paste described in the first aspect can be used in the HJT high efficiency cell.

[0040] In summary, compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects:

[0041] The low-temperature curing conductive silver paste for HJT high-efficiency batteries can be cured at low temperatures. In particular, when the adhesive resin is epoxy resin and the coupling agent is isopropyl tri(isostearoyl) titanate + isopropyl tri(dioctyl pyrophosphoryl) titanate, the low-temperature curing conductive silver paste has a sufficiently low resistivity (≤4×10-6 Ω·cm) after curing and a viscosity of 80~100 Pa.s, thereby obtaining better conductivity. At the same time, the inventor unexpectedly found that Re 2 O 7The addition of can prevent the excessive sintering of the silver-coated copper powder and the dendritic silver powder, which is conducive to the formation of excellent ohmic contact, thereby significantly improving the photoelectric conversion efficiency. Experiments have shown that when the low-temperature curing conductive silver paste provided by the present invention is used as a slurry for HJT high-efficiency batteries, it can produce excellent ohmic contact performance, show high conductivity and excellent photoelectric conversion efficiency, and is therefore particularly suitable for large-scale industrial production of HJT solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of a test line printed with a low-temperature curing conductive silver paste according to the present invention. DETAILED DESCRIPTION

[0043] The present invention is described in detail below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] According to the technical solution provided in the first aspect of the present invention, a low-temperature curing conductive silver paste for HJT high-efficiency batteries comprises the following components, measured in parts by mass: 63 parts of silver-coated copper powder, 13 parts of dendritic silver powder, 9 parts of coupling agent, 40 parts of organic carrier, and 4 parts of inhibitor; wherein the median particle size of the silver-coated copper powder is 85 nm, and the median particle size of the dendritic silver powder is 3 μm; the organic carrier is composed of an adhesive resin and an organic solvent, and the mass ratio of the adhesive resin to the organic solvent is 1:5.

[0045] In a preferred embodiment, a low-temperature curing conductive silver paste for HJT high-efficiency batteries comprises the following components, measured in parts by mass: 66 parts of silver-coated copper powder, 15 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 3 parts of inhibitor; wherein the median particle size of the silver-coated copper powder is 85 nm, and the median particle size of the dendritic silver powder is 5 μm; the organic carrier is composed of an adhesive resin and an organic solvent, and the mass ratio of the adhesive resin to the organic solvent is 1:5.

[0046] In another preferred embodiment, a low-temperature curing conductive silver paste for HJT high-efficiency batteries comprises the following components, measured in parts by mass: 68 parts of silver-coated copper powder, 20 parts of dendritic silver powder, 12 parts of coupling agent, 45 parts of organic carrier, and 5 parts of inhibitor; wherein the median particle size of the silver-coated copper powder is 70 nm, and the median particle size of the dendritic silver powder is 5 μm; the organic carrier is composed of an adhesive resin and an organic solvent, and the mass ratio of the adhesive resin to the organic solvent is 1:7.

[0047] In another preferred embodiment, a low-temperature curing conductive silver paste for HJT high-efficiency batteries comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 21 parts of dendritic silver powder, 13 parts of coupling agent, 45 parts of organic carrier, and 6 parts of inhibitor; wherein the median particle size of the silver-coated copper powder is 70 nm, and the median particle size of the dendritic silver powder is 6 μm; the organic carrier is composed of an adhesive resin and an organic solvent, and the mass ratio of the adhesive resin to the organic solvent is 1:6.

[0048] In some preferred embodiments, the coupling agent is selected from any one or more of the following combinations: isopropyl trioleyl titanate, isopropyl triisostearyl titanate, isopropyl tri(isooctanoyl) titanate, isopropyl dioleyl (dioctylphospho) titanate, isopropyl di(methacryloyl) isostearyl titanate, isopropyl tri(isostearoyl) titanate, and isopropyl tri(dioctyl pyrophospho) titanate.

[0049] In a preferred embodiment, the adhesive resin is an epoxy resin.

[0050] In another preferred embodiment, the adhesive resin is melamine urea-formaldehyde resin.

[0051] In yet another preferred embodiment, the adhesive resin is a phenolic resin.

[0052] In a further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is isopropyl titanate triisostearate.

[0053] In a further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is isopropyl dioleyloxy (dioctylphosphoyloxy) titanate.

[0054] In another further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is isopropyl di(methacryloyl) isostearyl titanate.

[0055] In another further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is a combination of isopropyl dioleyloxy (dioctylphosphoyloxy) titanate and isopropyl di(methacryloyl) isostearyl titanate.

[0056] In a further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is isopropyl tri(isostearoyl) titanate.

[0057] In a further preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is isopropyl tri(dioctylpyrophosphoryl) titanate.

[0058] In a most preferred embodiment, the adhesive resin is an epoxy resin, and the coupling agent is a combination of isopropyl tri(isostearoyl) titanate and isopropyl tri(dioctyl pyrophospho) titanate.

[0059] In some preferred embodiments, the organic solvent is selected from any one or more of the following combinations: terpineol, dihydroterpineol, ethylene glycol phenyl ether, propylene glycol phenyl ether, butyl carbitol, butyl carbitol acetate, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, dihydroterpineol acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0060] In a further preferred embodiment, the organic solvent consists of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether.

[0061] In a further preferred embodiment, the volume ratio of the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether is 1:2:1.

[0062] In another further preferred embodiment, the volume ratio of the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether is 1:1:1.

[0063] In another further preferred embodiment, the volume ratio of the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether is 2:1:1.

[0064] In yet another further preferred embodiment, the volume ratio of the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether is 1:1:2.

[0065] In a most preferred embodiment, the volume ratio of the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether is 2:1:2.

[0066] In a preferred embodiment, the organic carrier is prepared according to the following steps: first, the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether are uniformly mixed in a volume ratio of 1:1:1 to obtain a mixed solvent; then, a crude organic carrier solution is prepared according to the mixed solvent: epoxy resin = 6:1 (mass ratio); finally, heating in a water bath at 70-75°C while stirring for 0.5 hour, cooling to room temperature, and covering with plastic wrap to prevent solvent volatilization to obtain the organic carrier.

[0067] In another preferred embodiment, the organic carrier is prepared according to the following steps: first, the butyl carbitol, the diethylene glycol monoethyl ether and the diethylene glycol monobutyl ether are uniformly mixed in a volume ratio of 2:1:2 to obtain a mixed solvent; then, a crude organic carrier solution is prepared according to the mixed solvent: epoxy resin = 6:1 (mass ratio); finally, heating in a water bath at 70-75°C while stirring for 0.5 hour, cooling to room temperature, and covering with plastic wrap to prevent solvent volatilization to obtain the organic carrier.

[0068] In a preferred embodiment, the epoxy resin is diglycidyl 4,5-epoxycyclohexane-1,2-dicarboxylate.

[0069] In a preferred embodiment, the epoxy resin is diglycidyl hexahydrophthalate.

[0070] In a preferred embodiment, the epoxy resin is 1,2-epoxy-4-vinylcyclohexane.

[0071] In another preferred embodiment, the epoxy resin is a bisphenol A type epoxy resin.

[0072] In yet another preferred embodiment, the epoxy resin is a bisphenol S type epoxy resin.

[0073] In a most preferred embodiment, the epoxy resin is a bisphenol F type epoxy resin.

[0074] In a preferred embodiment, the inhibitor is Re 2 O 7 .

[0075] According to the technical solution provided in the second aspect of the present invention, the preparation method of the low-temperature curing conductive silver paste in the first aspect comprises the following steps:

[0076] S1: Weighing an adhesive resin and an organic solvent according to a certain mass ratio, adding the adhesive resin to the organic solvent, heating and stirring to obtain an organic carrier; the heating temperature is 160° C., and the heating duration is 35 minutes;

[0077] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0078] S3: subjecting the coarse mixed slurry to a vacuum degassing treatment; the vacuum degree of the vacuum degassing treatment is 0.12 MPa, and the duration of the vacuum degassing treatment is 20 minutes;

[0079] S4: grinding to obtain the low-temperature curing conductive silver paste.

[0080] In a preferred embodiment, the method for preparing the low temperature curing conductive silver paste comprises the following steps:

[0081] S1: Weighing an adhesive resin and an organic solvent according to a certain mass ratio, adding the adhesive resin to the organic solvent, heating and stirring to obtain an organic carrier; the heating temperature is 170° C., and the heating duration is 25 minutes;

[0082] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0083] S3: subjecting the coarse mixed slurry to vacuum degassing treatment; the vacuum degree of the vacuum degassing treatment is 0.10 MPa, and the duration of the vacuum degassing treatment is 16 minutes;

[0084] S4: grinding to obtain the low-temperature curing conductive silver paste.

[0085] In another preferred embodiment, the method for preparing the low temperature curing conductive silver paste comprises the following steps:

[0086] S1: weighing an adhesive resin and an organic solvent according to a certain mass ratio, adding the adhesive resin to the organic solvent, heating and stirring to obtain an organic carrier; the heating temperature is 190° C., and the heating duration is 15 minutes;

[0087] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0088] S3: subjecting the coarse mixed slurry to a vacuum degassing treatment; the vacuum degree of the vacuum degassing treatment is 0.08 MPa, and the duration of the vacuum degassing treatment is 12 minutes;

[0089] S4: grinding to obtain the low-temperature curing conductive silver paste.

[0090] The technical solution provided according to the third aspect of the present invention is the application of the low temperature curing conductive silver paste described in the first aspect in HJT high efficiency cells. Specifically, the HJT high efficiency cells use electrodes containing the low temperature curing conductive silver paste described in the first aspect.

[0091] The present invention is described in detail and specifically by specific examples below to provide a better understanding of the present invention, but the following examples do not limit the scope of the present invention.

[0092] Example 1

[0093] Prepare low temperature curing conductive silver paste I by following the steps below:

[0094] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0095] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0096] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0097] S4: After sufficient grinding at room temperature, a low-temperature curing conductive silver paste I is obtained.

[0098] The low-temperature curing conductive silver paste I comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 5 parts of inhibitor; the median particle size of the silver-coated copper powder is 60 nm, the median particle size of the dendritic silver powder is 4 μm; the inhibitor is Re 2 O 7 .

[0099] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0100] Wherein, the adhesive resin is bisphenol A epoxy resin, and the coupling agent is isopropyl tri(isostearoyl) titanate.

[0101] Example 2

[0102] Follow the steps below to prepare low temperature curing conductive silver paste II:

[0103] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0104] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0105] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0106] S4: After sufficient grinding at room temperature, a low-temperature curing conductive silver paste II is obtained.

[0107] The low temperature curing conductive silver paste II comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 5 parts of inhibitor; the median particle size of the silver-coated copper powder is 60 nm, the median particle size of the dendritic silver powder is 4 μm; the inhibitor is Re 2 O 7 .

[0108] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0109] Wherein, the adhesive resin is bisphenol S type epoxy resin, and the coupling agent is isopropyl tri(isostearoyl) titanate.

[0110] Example 3

[0111] Follow the steps below to prepare low temperature curing conductive silver paste III:

[0112] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0113] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0114] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0115] S4: After sufficient grinding at room temperature, a low-temperature curing conductive silver paste III is obtained.

[0116] The low temperature curing conductive silver paste III comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 5 parts of inhibitor; the median particle size of the silver-coated copper powder is 60 nm, the median particle size of the dendritic silver powder is 4 μm; the inhibitor is Re 2 O 7 .

[0117] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0118] Wherein, the adhesive resin is bisphenol F type epoxy resin, and the coupling agent is isopropyl tri(isostearoyl) titanate.

[0119] Example 4

[0120] In this embodiment, the coupling agent is isopropyl tri(dioctyl pyrophosphoryl) titanate; otherwise, the preparation steps and the types and proportions of the components are the same as those in Embodiment 3, and finally a low-temperature curing conductive silver paste IV is obtained.

[0121] Example 5

[0122] In this embodiment, the coupling agent is a combination of isopropyl tri(isostearoyl) titanate and isopropyl tri(dioctyl pyrophosphoryl) titanate (mass ratio 1:1); other than this, the preparation steps and the types and proportions of the components are the same as those in Example 3, and finally a low-temperature curing conductive silver paste V is obtained.

[0123] Example 6

[0124] Prepare low temperature curing conductive silver paste VI by following the steps below:

[0125] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0126] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0127] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0128] S4: After sufficient grinding at room temperature, a low-temperature curing conductive silver paste VI is obtained.

[0129] The low-temperature curing conductive silver paste VI comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 3 parts of inhibitor; the median particle size of the silver-coated copper powder is 60 nm, the median particle size of the dendritic silver powder is 4 μm; the inhibitor is Re 2 O 7 .

[0130] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0131] The adhesive resin is bisphenol F epoxy resin, and the coupling agent is a combination of isopropyl tri(isostearoyl) titanate and isopropyl tri(dioctyl pyrophosphoryl) titanate (mass ratio 1:1).

[0132] Example 7

[0133] In this embodiment, the added amount of the inhibitor is 4 parts by mass; otherwise, the preparation steps and the types and proportions of the components are the same as those in Embodiment 6, and finally a low-temperature curing conductive silver paste VII is obtained.

[0134] Example 8

[0135] In this embodiment, the added amount of the inhibitor is 6 parts by mass; other than this, the preparation steps and the types and proportions of the components are the same as those in Embodiment 6, and finally a low-temperature curing conductive silver paste VIII is obtained.

[0136] Comparative Example 1

[0137] Prepare the conductive silver paste α as follows:

[0138] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0139] S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0140] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0141] S4: After sufficient grinding at room temperature, a conductive silver paste α is obtained.

[0142] The conductive silver paste α comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, 42 parts of organic carrier, and 5 parts of inhibitor; the median particle size of the silver-coated copper powder is 60 nm, the median particle size of the dendritic silver powder is 4 μm; the inhibitor is Re 2 O 7 .

[0143] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0144] Wherein, the adhesive resin is bisphenol F epoxy resin, and the coupling agent is silane coupling agent Z-6040.

[0145] Comparative Example 2

[0146] In this comparative example, the coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane; except for this, the preparation steps and the types and proportions of the components are the same as those in comparative example 1, and finally a conductive silver paste β is prepared.

[0147] Comparative Example 3

[0148] Prepare the conductive silver paste γ as follows:

[0149] S1: At room temperature, weigh an adhesive resin and an organic solvent in a mass ratio of 1:6, add the adhesive resin to the organic solvent, heat at 170° C. for 25 minutes and stir to obtain an organic carrier;

[0150] S2: adding the silver-coated copper powder, the dendritic silver powder and the coupling agent to the organic carrier, stirring evenly to obtain a coarse mixed slurry;

[0151] S3: performing vacuum degassing treatment on the coarse mixed slurry at room temperature for 16 minutes (vacuum degree is 0.10 MPa);

[0152] S4: After sufficient grinding at room temperature, a conductive silver paste γ is obtained.

[0153] The conductive silver paste γ comprises the following components, in parts by mass: 70 parts of silver-coated copper powder, 16 parts of dendritic silver powder, 10 parts of coupling agent, and 42 parts of organic carrier; the median particle size of the silver-coated copper powder is 60 nm, and the median particle size of the dendritic silver powder is 4 μm.

[0154] Wherein, the organic solvent is composed of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether (volume ratio 2:1:2).

[0155] The adhesive resin is bisphenol F epoxy resin, and the coupling agent is a combination of isopropyl tri(isostearoyl) titanate and isopropyl tri(dioctyl pyrophosphoryl) titanate (mass ratio 1:1).

[0156] In addition, the inventors also tested the key indicators of low-temperature curing conductive silver pastes I~VIII and conductive silver pastes α~γ respectively.

[0157] Specifically, the viscosity of low-temperature curing conductive silver pastes I~VIII and conductive silver pastes α~γ was tested respectively. The test method was to use a viscometer to measure (Brookfiled SC4-1410rpm, 25℃), and a screen printer was used to print Brookfiled SC4-1410rpm, 25℃ on a 125mm×125mm Si substrate, and then sintered in a sintering furnace for 2-4 seconds. After sintering, an IV tester (HSC1-1S of Shanghai Heshuang Solar Technology Co., Ltd.) was used to test the electrical properties, and 40Sn / 60Pb was used for welding on the main grid line. The test results are shown in Table 1 below.

[0158] In addition, the resistivity tests were carried out on low temperature curing conductive silver pastes I~VIII and conductive silver pastes α~γ, mainly including:

[0159] The resistivity is calculated according to the formula ρ=RS / L; where ρ is the resistivity, L is the length of the material, S is the cross-sectional area of ​​the material, and R is the resistance value;

[0160] Before the resistivity test, the silver paste prepared in each embodiment was printed into the following Figure 1 The test lines shown are cured at 200°C for 30 minutes. The line width is 1.5mm and the length is 100mm. A laser microscope is used to test the film thickness of the lines at multiple points on the silver paste lines to obtain the average film thickness data. Secondly, the average film thickness data is multiplied by the line width (1.5mm) to obtain the cross-sectional area of ​​the line. The line length is a fixed value (100mm), and the R data is measured by a multimeter. Through calculation and unit conversion, the resistivity of the printed lines can be obtained. After averaging multiple lines, the average resistivity of the sample can be obtained; the test results are shown in Table 1 below.

[0161] In addition, the photoelectric conversion efficiency of the HJT electrodes containing low-temperature curing conductive silver pastes I to VIII and conductive silver pastes α to γ ​​were also tested; the test results are shown in Table 1 below.

[0162] Table 1

[0163]

[0164] It can be seen from Table 1 above that the conductive silver pastes α to γ ​​corresponding to Comparative Examples 1-3 exhibit lower photoelectric conversion efficiency; in particular, without adding the inhibitor Re 2 O 7 The photoelectric conversion efficiency of the conductive silver paste γ is the lowest (13.2%).

[0165] In contrast, Re 2 O 7 The addition of can prevent excessive sintering of silver-coated copper powder and dendritic silver powder, which is conducive to the formation of excellent ohmic contact, thereby significantly improving the photoelectric conversion efficiency. Therefore, the photoelectric conversion efficiency of low-temperature curing conductive silver pastes I~VIII is as high as 22.0~25.0%.

[0166] Moreover, it can be seen from Table 1 above that the resistivity detected from the conductive silver paste α and conductive silver paste β corresponding to Comparative Examples 1 and 2 are both relatively high. In significant contrast, the low-temperature curing conductive silver pastes V to VIII, in which the coupling agent is a combination of isopropyl tri(isostearoyl) titanate + isopropyl tri(dioctyl pyrophosphoryl) titanate, all exhibit extremely low resistivity, specifically in the range of 3.0×10-6 to 3.2×10-6, so the low-temperature curing conductive silver pastes V to VIII all have high conductivity.

[0167] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A low-temperature curing conductive silver paste for HJT high-efficiency batteries, characterized in that: The composition comprises the following components by weight: 60-72 parts of silver-coated copper powder, 12-24 parts of dendritic silver powder, 8-13 parts of coupling agent, 38-45 parts of organic carrier, and 3-6 parts of inhibitor; Wherein, the organic carrier is composed of an adhesive resin and an organic solvent; Wherein, the median particle size of the silver-coated copper powder is 55-90nm; Among them, the median particle size of the dendritic silver powder is 3-6 μm; The inhibitor is Re2O7; Wherein, the coupling agent is selected from any one or more of the following combinations: isopropyl trioleyl titanate, isopropyl triisostearyl titanate, isopropyl tri(isooctanoyl) titanate, isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl di(methacryloyl) isostearyl titanate, isopropyl tri(isostearoyl) titanate, and isopropyl tri(dioctyl pyrophosphoryl) titanate.

2. The low temperature curing conductive silver paste according to claim 1, characterized in that: The mass ratio of the adhesive resin to the organic solvent is 1:5 to 1:

8.

3. The low temperature curing conductive silver paste according to claim 1, characterized in that: The adhesive resin is selected from any one or more combinations of the following: epoxy resin, acrylic resin, phenolic resin, and melamine urea-formaldehyde resin.

4. The low temperature curing conductive silver paste according to claim 1, characterized in that: The organic solvent is selected from any one or more of the following combinations: terpineol, dihydroterpineol, ethylene glycol phenyl ether, propylene glycol phenyl ether, butyl carbitol, butyl carbitol acetate, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, dihydroterpineol acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

5. The low temperature curing conductive silver paste according to claim 4, characterized in that: The organic solvent consists of butyl carbitol, diethylene glycol monoethyl ether and diethylene glycol monobutyl ether.

6. A method for preparing a low temperature curing conductive silver paste according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: weighing an adhesive resin and an organic solvent according to a certain mass ratio, adding the adhesive resin into the organic solvent, heating and stirring to obtain an organic carrier; S2: adding the silver-coated copper powder, the dendritic silver powder, the coupling agent and the inhibitor to the organic carrier, stirring evenly to obtain a coarse mixed slurry; S3: subjecting the coarse mixed slurry to vacuum degassing treatment; and S4: grinding to obtain the low-temperature curing conductive silver paste.

7. The preparation method according to claim 6, characterized in that: In S1, the heating temperature is 160-190° C., and the heating duration is 15-35 minutes.

8. The preparation method according to claim 6, characterized in that: In S3, the vacuum degree of the vacuum degassing treatment is 0.08-0.12 MPa, and the duration of the vacuum degassing treatment is 12-20 minutes.

Citation Information

Patent Citations

  • Positive silver paste and preparation method thereof

    CN107068241A

  • Organic silicon resin conductive adhesive, and preparation method therefor and application thereof

    CN113412321A

  • Low-temperature conductive paste composition, preparation method and application thereof

    CN113963840A