A method for preparing tungsten alloy composite powder

By doping Zr elements in the preparation process of tungsten alloy composite powder, forming ZrO2 or Er-Zr-O structure, refining the particle size and absorbing oxygen impurities, the problem of the influence of particle size and oxygen impurities of tungsten alloy composite powder is solved, and the problem of particle size and oxygen impurities of tungsten alloy composite powder is improved, The stability and mechanical properties of the material are achieved, and low-cost and efficient preparation of tungsten alloy composite powder is achieved.

CN114985752BActive Publication Date: 2024-11-15BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210455800.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-11-15
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

In the prior art, the particle size of the tungsten alloy composite powder cannot be effectively refined, and oxygen impurities affect their performance, resulting in insufficient brittleness and toughness, limiting their wide application.

Method used

During the preparation of W-Er2O3 composite powder, trace amounts of Zr elements are doped, and ZrO2 or Er-Zr-O structure is formed through co-deposition reaction, which hinders the growth of W particles and absorbs free oxygen, and further refines the W-Zr-Er2O3 composite powder. and a small size tungsten alloy composite powder was obtained by calcining and reduction.

Benefits of technology

The particle size of the tungsten alloy composite powder is significantly reduced, and the oxide particles are uniformly distributed, which improves the stability and mechanical properties of the material, reduces costs, and provides the possibility of oxide dispersion strengthening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114985752B_ABST
    Figure CN114985752B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of nano-scale materials, and in particular to a method for preparing tungsten alloy composite powder. The method comprises: using dehydrated ammonium paratungstate, erbium element compounds and zirconium element compounds as raw materials, mixing them under acidic conditions by a co-precipitation method to obtain a precursor of a tungsten alloy composite material; the molar ratio of the erbium element compound in the erbium salt to the zirconium element in the zirconium element compound is 1:(0.5-5). The present invention uses ammonium paratungstate, erbium element compounds and zirconium element compounds as raw materials to prepare tungsten alloy composite powder. The doping of zirconium element can hinder the growth of W particles and absorb free oxygen, and the particle size of the prepared tungsten alloy composite powder is reduced to 100-200nm. The preparation method provided by the present invention is simple and highly operable, and has excellent performance in the field of preparing oxide dispersion enhanced tungsten alloy powder, and is expected to be widely used as a plasma surface material in a fusion reactor in the field of high-temperature applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano-level materials, and in particular to a method for preparing tungsten alloy composite powder. Background Art

[0002] Tungsten alloy has excellent properties such as high melting point, high thermal conductivity, high density, low thermal expansion coefficient, low vapor pressure, low tritium retention and low thermal expansion coefficient. It is widely used in military, nuclear reactors and spacecraft equipment, and is considered to be the most promising plasma-facing first wall material.

[0003] However, tungsten alloys are limited in their wide application due to their inherent low-temperature brittleness, high ductile-brittle transition temperature, recrystallization brittleness, and neutron irradiation brittleness. In order to improve the brittleness of tungsten and its mechanical properties, the existing technology dopes a small amount of simple oxides such as Er2O3 into the tungsten matrix to hinder the growth of W particles during the reduction process, thereby refining the W particles. However, the size of the composite powder obtained is micron-level and the influence of oxygen impurities cannot be effectively removed, which has an adverse effect on the performance of tungsten alloys. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a method for preparing tungsten alloy composite powder, by doping zirconium element in the preparation process of W-Er2O3 composite powder through co-deposition reaction, further refining the particle size of W-Er2O3 composite powder, and making the whole system more stable.

[0005] In a first aspect, the present invention provides a method for preparing a tungsten alloy composite powder, comprising:

[0006] Dehydrated ammonium paratungstate, erbium element compound and zirconium element compound are used as raw materials, and a precursor of tungsten alloy composite powder is obtained by co-precipitation method under acidic conditions.

[0007] The molar ratio of the erbium element compound in the erbium salt to the zirconium element in the zirconium element compound is 1:(0.5-5).

[0008] The present invention dopes Zr in the preparation process of W-Er2O3 composite powder. Doping with trace Zr can hinder the growth of W particles, and Zr reacts with free oxygen to form a stable ZrO2 or Er-Zr-O structure, which can effectively absorb free oxygen, ultimately making the size of the W-Zr-Er2O3 composite powder significantly reduced, and the doped oxide particles are also more evenly distributed.

[0009] Furthermore, the molar ratio of the tungsten element in the dehydrated ammonium paratungstate to the erbium element in the erbium element compound is 1:1 to 1:3.

[0010] Furthermore, the erbium element compound includes one or more of Er2O3, Er(NO3)3, ErCl3 or ErF3; the zirconium element compound includes one or more of ZrOCl2, ZrO2, ZrH2 or ZrO(NO3)2.

[0011] Furthermore, it also includes:

[0012] The precursor of the tungsten alloy composite powder is calcined and reduced to obtain the tungsten alloy composite powder.

[0013] Further, the calcination comprises: calcining at 500-600° C. for 2-3 hours;

[0014] The reduction is carried out at 600-700° C. for 3-4 hours, and then at 800-900° C. for 6-7 hours.

[0015] Furthermore, the dehydrated ammonium paratungstate is prepared by the following method:

[0016] Ammonium paratungstate is calcined at 150-200°C for 1.5-2 hours.

[0017] Further, the co-deposition reaction comprises:

[0018] After the raw materials are mixed, the pH is adjusted to less than 1 by acid, and after reacting for 30 to 45 minutes, anhydrous ethanol is added and the reaction is continued for 3 to 4 hours, and then filtered and dried to obtain the precursor of the tungsten alloy composite powder.

[0019] Further, the drying comprises:

[0020] Dry at 60-70°C for 12-14 hours.

[0021] As a preferred specific embodiment, the present invention provides a method for preparing tungsten alloy composite powder, comprising:

[0022] Calcine ammonium paratungstate at 150-200°C for 1.5-2 hours to obtain dehydrated ammonium paratungstate;

[0023] Dehydrated ammonium paratungstate, erbium element compound and zirconium element compound are mixed as raw materials, pH is adjusted to less than 1 by acid, after reacting for 30 to 45 minutes, anhydrous ethanol is added to continue reacting for 3 to 4 hours, and then filtered and dried to obtain the precursor of the tungsten alloy composite powder;

[0024] The precursor of the tungsten alloy composite powder is calcined at 500-600° C. for 2-3 hours, then treated at 600-700° C. for 3-4 hours, and then treated at 800-900° C. for 6-7 hours to obtain the tungsten alloy composite powder.

[0025] In a second aspect, the present invention provides tungsten alloy composite powder prepared by the method.

[0026] The present invention has the following beneficial effects:

[0027] The present invention uses APT, erbium element compound and zirconium element compound as raw materials, prepares the precursor of tungsten alloy composite powder by co-precipitation under acidic conditions, and obtains small-sized W-Zr-Er2O3 composite powder by calcination and reduction. Compared with W-Er2O3 composite powder prepared under the same conditions, the size of W-Zr-Er2O3 composite powder is significantly reduced because the doping of trace Zr hinders the growth of W particles and absorbs free oxygen in W, and the doped oxide particles are evenly distributed. The method provided by the present invention can simply and efficiently prepare small-sized W-Zr-Er2O3 composite powder, does not need to be ultrasonically treated, has low cost and strong repeatability, and provides a good reference for the later preparation of oxide dispersion-strengthened tungsten alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the XRD result of the precursor powder prepared in Example 1 of the present invention.

[0029] Figure 2 This is a SEM image of the precursor powder prepared in Example 1 of the present invention.

[0030] Figure 3 This is the XRD result of the calcined powder prepared in Example 1 of the present invention.

[0031] Figure 4 This is a SEM image of the calcined powder prepared in Example 1 of the present invention.

[0032] Figure 5 This is the XRD result of the reduced powder prepared in Example 1 of the present invention.

[0033] Figure 6 These are SEM images of the reduced powders prepared in Examples 1 and 2 of the present invention; the two images on the left are SEM images of the reduced powders prepared in Example 1, and the two images on the right are SEM images of the reduced powders prepared in Example 2.

[0034] Figure 7 This is the EDS energy spectrum of the reduced powder prepared in Example 1 of the present invention.

[0035] Figure 8 The SEM image of the precursor powder prepared in Experimental Example 1 of the present invention; the left image is the SEM image of the precursor powder prepared in Example 1, and the right image is the SEM image of the precursor powder prepared in Example 2.

[0036] Fig. 9 The SEM image of the calcined powder prepared in Experimental Example 1 of the present invention; the left image is the SEM image of the calcined powder prepared in Example 1, and the right image is the SEM image of the calcined powder prepared in Example 2. DETAILED DESCRIPTION

[0037] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0038] Example 1

[0039] This embodiment provides a method for preparing nano-scale tungsten alloy composite powder, and the specific formula is as follows:

[0040] Table 1 Composition of tungsten alloy composite powder

[0041]

[0042] When the volume fraction of Er2O3 is set to 2%, the Er2Zr2O7 dispersed phase is expected to be generated at a molar ratio of [Er]:[Zr]=1:1, so the preferred mass fraction of Zr is 0.43%.

[0043] APT was calcined in a muffle furnace at 150°C for 1.5h for dehydration, 1.1g Er(NO3)3·6H2O and 0.77g ZrOCl2·8H2O were weighed and dissolved in 430mL deionized water, 70.12g dehydrated APT was added to the prepared solution, the water bath magnetic stirrer was turned on and the control temperature was adjusted to 25°C, the stirring rate was 300rpm, and a magnet was placed in a beaker and placed in a water bath magnetic stirrer and mechanically stirred to fully dissolve and disperse it.

[0044] Then, 54 mL of concentrated nitric acid was added to the beaker to adjust the pH (pH < 1) to initiate the co-precipitation reaction. After about 30 minutes of reaction, 500 mL of anhydrous ethanol was added and the reaction was continued for 3 hours to slow down the deposition of tungstic acid and allow it to react fully.

[0045] After the reaction is completed, stirring is stopped, the prepared precursor powder is vacuum filtered in a vacuum filter, the drying oven is opened and the temperature is adjusted to 60°C, and the filtered powder is placed in the drying oven and dried for 12 hours.

[0046] The X-ray diffraction results of the precursor powder are as follows: Figure 1 The scanning electron microscopy results are shown in Figure 2 shown.

[0047] After the precursor powder was fully ground in a mortar, the powder was placed in a muffle furnace and calcined at 500 °C for 2 h.

[0048] After calcination, the X-ray diffraction results of the powder are as follows Figure 3 The scanning electron microscopy results are shown in Figure 4 shown.

[0049] Finally, the calcined powder was reduced in a tube furnace at 650°C / 3h+850°C / 6h to obtain W-Zr-Er2O3 composite powder.

[0050] The X-ray diffraction results of the obtained W-Zr-Er2O3 composite powder are as follows: Figure 5 The scanning electron microscopy results are shown in Figure 6 shown.

[0051] The EDS spectrum of the obtained W-Zr-Er2O3 composite powder is as follows: Figure 7 shown.

[0052] Example 2

[0053] This embodiment provides a method for preparing micron-sized tungsten alloy composite powder, and the specific formula is as follows:

[0054] Table 2 Composition of tungsten alloy composite powder

[0055]

[0056] APT was calcined in a muffle furnace at 150°C for 1.5h for dehydration, 1.1g Er(NO3)3·6H2O was weighed and dissolved in 430mL deionized water, 70.12g dehydrated APT was added to the prepared solution, the water bath magnetic stirrer was turned on and the control temperature was adjusted to 25°C, the stirring rate was 300rpm, and a magnet was placed in a beaker and placed in a water bath magnetic stirrer and mechanically stirred to fully dissolve and disperse it.

[0057] Then, 54 mL of concentrated nitric acid was added to the beaker to adjust the pH (pH < 1) to initiate the co-precipitation reaction. After about 30 minutes of reaction, 500 mL of anhydrous ethanol was added and the reaction was continued for 3 hours to slow down the deposition of tungstic acid and allow it to react fully.

[0058] After the reaction is completed, stop stirring, vacuum filter the prepared precursor powder in a vacuum filter, open the drying oven and adjust the temperature to 60°C, and put the filtered powder into the drying oven to dry for 12 hours. After the precursor powder is fully ground in a mortar, the powder is placed in a muffle furnace and calcined at 500°C for 2 hours. Finally, the calcined powder is reduced in a tube furnace at 650°C / 3h+850°C / 6h to obtain W-Er2O3 composite powder. The electron microscope scanning results are as follows: Figure 6 shown.

[0059] Test Example 1

[0060] This test example compares the morphology and performance of the W-Zr-Er2O3 composite powder prepared in Example 1 and the W-Er2O3 composite powder prepared in Example 2, and compares the morphology images of the precursor powder, calcined powder and reduced powder of the two.

[0061] from Figure 8 The results show that the W-Zr-Er2O3 precursor powder has two different morphologies: one is a micron-scale flake structure, and the other is a nano-sphere. The W-Er2O3 precursor powder is an unevenly agglomerated sphere, and is larger than the nano-sphere in the W-Zr-Er2O3 composite powder.

[0062] from Fig. 9 The results shown show that the flake structure in the W-Zr-Er2O3 calcined powder decomposes and forms nano-spheres, and the size of the nano-spheres is smaller than that of the W-Er2O3 calcined powder.

[0063] from Figure 6 The results shown show that both the 100nm electron microscope scanning image and the 300nm electron microscope scanning image show that the particle size of the W-Zr-Er2O3 composite powder is significantly smaller than that of the W-Er2O3 composite powder. The particle size of the W-Zr-Er2O3 composite powder is generally between 50nm and 300nm, and the particle size of the W-Er2O3 composite powder is generally between 300nm and 600nm. At the same time, the oxide particles are evenly distributed on the surface of the W-Zr-Er2O3 composite powder, and the oxide particles in the W-Er2O3 composite powder show agglomeration.

[0064] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing tungsten alloy composite powder, It is characterized in that include: Dehydrated ammonium paratungstate, erbium element compound and zirconium element compound are used as raw materials, mixed and adjusted to pH less than 1 by acid, reacted for 30 to 45 minutes, added with anhydrous ethanol and continued to react for 3 to 4 hours, then filtered and dried to obtain a precursor of tungsten alloy composite powder; the precursor of tungsten alloy composite powder is calcined and reduced to obtain tungsten alloy composite powder; The molar ratio of the erbium element in the erbium element compound to the zirconium element in the zirconium element compound is 1:(0.5-5).

2. The method according to claim 1, It is characterized in that The molar ratio of the tungsten element in the dehydrated ammonium paratungstate to the erbium element in the erbium element compound is 1:1 to 1:

3.

3. The method according to claim 1, It is characterized in that The erbium element compound includes Er 2 O 3 、Er(NO 3 ) 3 、ErCl 3 or ErF 3 One or more of; and / or, the zirconium compound includes ZrOCl 2 、ZrO 2 , ZrH 2 or ZrO(NO 3 ) 2 One or more of .

4. The method according to claim 1, It is characterized in that The calcination comprises: calcining at 500-600° C. for 2-3 hours; The reduction is carried out at 600-700° C. for 3-4 hours, and then at 800-900° C. for 6-7 hours.

5. The method according to claim 1, It is characterized in that The dehydrated ammonium paratungstate is prepared by the following method: Ammonium paratungstate is calcined at 150-200°C for 1.5-2 hours.

6. The method according to claim 1, It is characterized in that The drying comprises: Dry at 60-70°C for 12-14 hours.

7. Tungsten alloy composite powder prepared by the method according to any one of claims 1 to 6.

8. Use of the tungsten alloy composite powder according to claim 7 as a plasma surface material in a fusion reactor.