Polyethylene resin composition and molded article

By optimizing the composition of ultra-high molecular weight polyethylene powder and metal soap, and adjusting the viscosity-average molecular weight and twin-screw extrusion conditions, the problem of fouling during the polyethylene resin molding process was solved, thereby improving the voltage resistance of the battery separator and the safety of the battery.

CN114989512BActive Publication Date: 2024-11-26ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210189023.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-02
Filing Date
2022-02-28
Publication Date
2024-11-26
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

In the prior art, polyethylene resin is prone to scale buildup on the die lip of the extruder during the molding process, resulting in poor appearance and reduced quality of the molded body. At the same time, the additives in metal soap can also cause scale buildup and residue, affecting the voltage resistance performance of the battery separator.

Method used

By controlling the composition of ultra-high molecular weight polyethylene powder and metal soap, adjusting the viscosity-average molecular weight and twin-screw extrusion conditions, optimizing the aspect ratio of the wire stock, reducing metal soap buildup and residue, and improving the quality and voltage resistance of the molded product.

Benefits of technology

It effectively inhibits the accumulation and residue of metal soap, improves the quality of the molded body and the voltage resistance of the battery separator, and enhances battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114989512B_ABST
    Figure CN114989512B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyethylene resin composition and a molded body. The present invention provides a polyethylene resin composition that suppresses the amount of scale from metal soap, suppresses the amount of metal soap residue, can improve the withstand voltage of the diaphragm, and can improve the safety of the battery. A polyethylene resin composition, wherein the polyethylene resin composition contains ultra-high molecular weight polyethylene powder and metal soap, the viscosity average molecular weight of the polyethylene resin composition is 100,000 to 10,000,000, and the longitudinal / lateral ratio of the strand deposit when the polyethylene resin composition is twin-screw extruded under specified conditions is greater than 0.05 and less than 7.0. <Twin-screw extrusion conditions> Polymer concentration: According to the viscosity average molecular weight (Mv) of the polyethylene resin composition, the polymer concentration is adjusted to be greater than the value of Formula I and less than the value of Formula II. Formula I: Y = 260.63X ‑0.484 , Y: polymer concentration, X: molecular weight (Mv); Formula II: Y = 338.69X ‑0.626 , Y: polymer concentration, X: molecular weight (Mv). Polyethylene resin composition: 5% to 50% by mass; liquid paraffin: 50% to 95% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyethylene resin composition and a molded body. Background Art

[0002] Polyethylene is used for various purposes such as sheets, films, and molded products, and one of its important uses is as a raw material for battery separators (hereinafter, sometimes referred to as separator raw materials).

[0003] The separator is a porous membrane used mainly to separate the positive electrode and the negative electrode inside the battery and to allow only ions to pass through.

[0004] Other uses of the above-mentioned separator include: use as a component of a battery for ensuring sufficient strength for practical use of the battery, use as a component that performs a shutdown (hereinafter also referred to as "fuse") function for preventing runaway battery reaction when the temperature inside the battery reaches a high level, etc.

[0005] As polyethylene used as a raw material for a separator, polyethylene having a higher molecular weight and a higher density than general-purpose polyethylene used for sheets, films, molded bodies, etc. is generally used, and is manufactured into a product in a powder form.

[0006] The reason why polyethylene, which is a raw material of the separator, has a high molecular weight and a high density is to ensure the strength of the separator.

[0007] The reason why polyethylene, which is a raw material of the separator, is in a powdery form is that it has poor processability due to its high molecular weight and is difficult to form into pellets, and also because a powdery form is more excellent in processability of the separator.

[0008] Conventionally, it has been known that, in the process of molding a molded product such as a diaphragm, when polyethylene and liquid paraffin are kneaded and extruded, a phenomenon in which deposits are attached to the die lip of the extruder is known.

[0009] Generally, fouling in the molding process refers to the accumulation of resin and the like on the die lip of the extruder over time due to continuous extrusion molding. The fouling adheres to the molded product, causing problems such as poor appearance. As a countermeasure in this case, the following treatment is performed: temporarily stop the operation of the molding machine, remove the accumulated fouling, and then restart the operation. Therefore, there is a problem that long-term continuous molding processing cannot be performed, the workability is reduced, and the quality of the molded product is also reduced.

[0010] As a method for reducing such fouling, a method of adding a metal soap such as calcium stearate and zinc stearate to a resin composition at a predetermined mass ratio is known (for example, see Patent Document 1).

[0011] Prior art literature

[0012] Patent Literature

[0013] [Patent Document 1] Japanese Patent Application Publication No. 2001-310987 Summary of the invention

[0014] Problems to be solved by the invention

[0015] The above-mentioned fouling includes fouling derived from resin and fouling derived from metal soap added as an additive.

[0016] When a molded article made of polyethylene is molded, both the depositing from the resin and the depositing from the metal soap become problems, and reduction of these deposits is required.

[0017] Although the technology described in Patent Document 1 has the effect of suppressing the amount of fouling from the resin, it has not studied the amount of fouling from the metal soap. In addition, from the perspective of improving the quality of the separator (less foreign matter in the battery), it is preferred that the amount of metal soap as an additive remaining in the molded body, especially the separator, is small.

[0018] Furthermore, in recent years, in order to improve the safety of batteries, it has been required to increase the withstand voltage of separators.

[0019] Therefore, an object of the present invention is to suppress the amount of scale deposited from metal soap and the amount of metal soap remaining as residue in a molded body, thereby improving the quality of the molded body and increasing the withstand voltage of a separator as a molded body, thereby improving battery safety.

[0020] Means used to solve problems

[0021] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that, in a polyethylene resin composition comprising an ultra-high molecular weight polyethylene powder and a metal soap, the above-mentioned problems can be solved by specifying the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene powder and the aspect ratio of the strands when the polyethylene resin composition is twin-screw extruded under specific conditions, thereby completing the present invention.

[0022] In addition, it was found that in a polyethylene resin composition comprising ultra-high molecular weight polyethylene powder and a metal soap, the above-mentioned problems can be solved by specifying the viscosity average molecular weight (Mv) of the polyethylene resin composition and the average number of carbon atoms per alkyl chain of the metal soap, thereby completing the present invention.

[0023] That is, the present invention is as follows. [1]

[0025] A polyethylene resin composition, comprising ultra-high molecular weight polyethylene powder and metal soap, wherein:

[0026] The viscosity average molecular weight (Mv) of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and

[0027] When the polyethylene resin composition is subjected to twin-screw extrusion under the following <Twin-screw extrusion conditions>, the aspect ratio of the strand deposit is vertical / horizontal=0.05 or more and 7.0 or less,

[0028] <Twin-screw extrusion conditions>

[0029] Polymer concentration: According to the viscosity average molecular weight (Mv) of the polyethylene resin composition,

[0030] The polymer concentration is adjusted to be above the value of formula I and below the value of formula II,

[0031] Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight (Mv)

[0032] Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight (Mv)

[0033] Polyethylene resin composition: 5% to 50% by mass

[0034] Liquid paraffin: 50% to 95% by mass

[0035] Extruder: Counter-rotating twin-screw extruder

[0036] Extrusion temperature: 160℃

[0037] Screw speed: 150rpm

[0038] The diameter of the discharge port: 1.0mm

[0039] Addition amount of metal soap: Add 5% of metal soap relative to the mass of ultra-high molecular weight polyethylene powder

[0040] Height from outlet to ground: 1.0m or more and 1.1m or less

[0041] Discharge: 0.5kg / hour or more and 5.0kg / hour or less

[0042] Squeeze time: 1 hour

[0043] Atmospheric temperature and humidity: 15°C or higher and 30°C or lower, 20%RH or higher and 70%RH or lower

[0044] Table material: aluminum plate. [2]

[0046] The polyethylene resin composition as described in the above [1], wherein the discharge rate under the twin-screw extrusion conditions is 2.0 kg / hour to 3.0 kg / hour. [3]

[0048] The polyethylene resin composition as described in the above [1] or [2], wherein the discharge rate under the twin-screw extrusion conditions is 2.5 kg / hour. [4]

[0050] The polyethylene resin composition as described in any one of [1] to [3] above, wherein the content of the metal soap is 0.01 mass % or more and 0.3 mass % or less. [5]

[0052] The polyethylene resin composition as described in any one of [1] to [4] above, wherein the average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 28.0 or less. [6]

[0054] The polyethylene resin composition as described in any one of [1] to [5] above, wherein the metal soap contains a fatty acid having 16 carbon atoms per alkyl chain and a fatty acid having 18 carbon atoms per alkyl chain (C16, C18), and

[0055] The mass ratio of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain (C18 / C16) is 1.5 or more and 1,000 or less. [7]

[0057] The polyethylene resin composition according to any one of [1] to [6] above, wherein the Ca ion concentration of the metal soap is 1.0 mg / L or more and 200 mg / L or less. [8]

[0059] The polyethylene resin composition as described in any one of [1] to [7] above, wherein the metal soap contains 0.1% by mass or more and 2.0% by mass or less of a fatty acid having 16 or 18 carbon atoms. [9]

[0061] A molded article, wherein the molded article is a molded article of the polyethylene resin composition according to any one of [1] to [8] above.

[10]

[0063] The molded body as described in the above [9], wherein the molded body is any one selected from the group consisting of a microporous film, a high-strength fiber, and a sintered body.

[11]

[0065] A polyethylene resin composition, comprising ultra-high molecular weight polyethylene powder and metal soap, wherein:

[0066] The viscosity average molecular weight (Mv) of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and

[0067] The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 28.0 or less.

[12]

[0069] The polyethylene resin composition according to the above

[11] , wherein the content of the metal soap is 0.01 mass % to 0.3 mass %.

[13]

[0071] The polyethylene resin composition as described in

[11] or

[12] above, wherein the metal soap contains a fatty acid having 16 carbon atoms per alkyl chain and a fatty acid having 18 carbon atoms per alkyl chain (C16, C18), and

[0072] The mass ratio of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain (C18 / C16) is 1.5 or more and 1,000 or less.

[14]

[0074] The polyethylene resin composition according to any one of

[11] to

[13] above, wherein the Ca ion concentration of the metal soap is 1.0 mg / L or more and 200 mg / L or less.

[15]

[0076] The polyethylene resin composition as described in any one of

[11] to

[14] above, wherein the content of the fatty acid having 16 or 18 carbon atoms in the metal soap is 0.1 mass % or more and 2.0 mass % or less.

[16]

[0078] A molded article, wherein the molded article is a molded article of the polyethylene resin composition according to any one of

[11] to

[15] above.

[17]

[0080] The molded body as described in the above

[16] , wherein the molded body is any one selected from the group consisting of a microporous film, a high-strength fiber, and a sintered body.

[0081] Effects of the Invention

[0082] According to the present invention, the amount of scale deposited from metal soap can be suppressed, and the amount of metal soap remaining as residue in the molded body can be suppressed, the quality of the molded body can be improved, and the withstand voltage of the separator as the molded body can be increased, thereby improving the safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] Figure 1 This is an explanatory diagram showing a method for measuring the longitudinal and transverse directions of a strand deposit. DETAILED DESCRIPTION

[0084] Hereinafter, the mode for implementing the present invention (hereinafter referred to as "this embodiment") is described in detail. It should be noted that this embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following contents. The present invention can be implemented after various modifications within the scope of its purpose.

[0085] [Polyethylene resin composition]

[0086] The polyethylene resin composition of the present embodiment contains ultrahigh molecular weight polyethylene powder and metal soap. In addition, in this specification, a processed product obtained by processing the polyethylene resin composition using an extruder or the like is also referred to as the polyethylene resin composition.

[0087] In the polyethylene resin composition of the first embodiment, the viscosity average molecular weight (Mv) of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and

[0088] When the polyethylene resin composition is subjected to twin-screw extrusion under the following <Twin-screw extrusion conditions>, the aspect ratio of the strand deposit is vertical / horizontal=0.05 or more and 7.0 or less.

[0089] <Twin-screw extrusion conditions>

[0090] Polymer concentration: According to the viscosity average molecular weight (Mv) of the polyethylene resin composition,

[0091] The concentration of the polymer is adjusted to be greater than the value of the following formula I and less than the value of the following formula II.

[0092] Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight (Mv)

[0093] Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight (Mv)

[0094] Polyethylene resin composition: 5% to 50% by mass

[0095] Liquid paraffin: 50% to 95% by mass

[0096] Extruder: Counter-rotating twin-screw extruder

[0097] Extrusion temperature: 160℃

[0098] Screw speed: 150rpm

[0099] The diameter of the discharge port: 1.0mm

[0100] Addition amount of metal soap: Add 5% of metal soap relative to the mass of ultra-high molecular weight polyethylene powder

[0101] Height from outlet to ground: 1.0m or more and 1.1m or less

[0102] Discharge: 0.5kg / hour or more and 5.0kg / hour or less

[0103] Squeeze time: 1 hour

[0104] Atmospheric temperature and humidity: 15°C or higher and 30°C or lower, 20%RH or higher and 70%RH or lower

[0105] Table material: Aluminum plate

[0106] The polyethylene resin composition of the second embodiment is a polyethylene resin composition containing an ultra-high molecular weight polyethylene powder and a metal soap, wherein:

[0107] The viscosity average molecular weight (Mv) of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and

[0108] The metal soap contains an alkyl chain, and the average number of carbon atoms per one of the alkyl chains is 16.0 or more and 28.0 or less.

[0109] Hereinafter, the polyethylene resin composition of the first embodiment and the polyethylene resin composition of the second embodiment may be collectively described as the polyethylene resin composition of the present embodiment.

[0110] By having the above-mentioned structure, the following effects can be achieved: the amount of scale from metal soap can be suppressed, and the amount of metal soap remaining as residue in the molded body can be suppressed, the quality of the molded body can be improved, and the withstand voltage of the separator as the molded body can be improved, thereby improving the safety of the battery.

[0111] (Ultra-high molecular weight polyethylene powder)

[0112] From the viewpoint of moldability and final physical properties, the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene powder (hereinafter, also referred to as “powder”) used in the polyethylene resin composition of the present embodiment is 10×10 4Above and 1000×10 4 the following.

[0113] In addition, from the viewpoint of moldability and final physical properties, the viscosity average molecular weight (Mv) of the ultrahigh molecular weight polyethylene powder is preferably 10×10 4 Above and 900×10 4 Below, more preferably 10×10 4 Above and 800×10 4 Below, more preferably 10×10 4 Above and 500×10 4 the following.

[0114] The viscosity average molecular weight (Mv) is a value obtained by converting the intrinsic viscosity obtained from the specific viscosity of the polymer solution into the viscosity average molecular weight. Specifically, the viscosity average molecular weight can be obtained by the method described in the examples described below.

[0115] The ultra-high molecular weight polyethylene powder may be any of a powder containing an ethylene homopolymer and a powder containing a copolymer of ethylene and an olefin copolymerizable with ethylene (hereinafter also referred to as a comonomer) (hereinafter also referred to as an ethylene-based polymer).

[0116] Examples of the olefin copolymerizable with ethylene include α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, and olefins of the formula CH2=CHR 1 (Here, R 1 The present invention may be a comonomer selected from the group consisting of a compound represented by an aryl group having 6 to 12 carbon atoms, and a linear, branched or cyclic diene having 3 to 15 carbon atoms, but is not limited thereto.

[0117] Among them, α-olefins having 3 to 15 carbon atoms are preferred.

[0118] Examples of the α-olefin include, but are not limited to, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.

[0119] When the ultra-high molecular weight polyethylene powder contains a comonomer as an olefin copolymerizable with ethylene, the content of the comonomer unit is preferably 0.01 mol% or more and 5 mol% or less, more preferably 0.01 mol% or more and 2 mol% or less, and further preferably 0.01 mol% or more and 1 mol% or less. It should be noted that, from the viewpoint of suppressing the decomposition rate, the comonomer amount is preferably set to 5 mol% or less.

[0120] <Viscosity average molecular weight>

[0121] As mentioned above, the viscosity average molecular weight (Mv) of the polyethylene resin composition is 10×10 4 Above and 1000×10 4 Below, preferably 10×10 4 Above and 900×10 4 Below, more preferably 10×10 4 Above and 800×10 4 Below, more preferably 10×10 4 Above and 500×10 4 the following.

[0122] The viscosity average molecular weight (Mv) of the polyethylene resin composition is 10×10 4 The strength of the polyethylene resin composition is further improved. In addition, the viscosity average molecular weight (Mv) of the polyethylene resin composition is 1000×10 4 Next, the moldability of the polyethylene resin composition is further improved.

[0123] When the polyethylene resin composition of the present embodiment is used for a molded product such as a diaphragm, the viscosity average molecular weight (Mv) of the polyethylene resin composition is preferably 10×10 4 Above and less than 300×10 4 , more preferably 10×10 4 Above and 200×10 4 When the polyethylene resin composition of the present embodiment is used for a molded product such as a high-strength fiber, the viscosity average molecular weight (Mv) of the polyethylene resin composition is preferably 300×10 4 Above and 1000×10 4 Below, more preferably 300×10 4 Above and 800×10 4 the following.

[0124] It should be noted that the viscosity average molecular weight of the polyethylene resin composition of the present embodiment shows substantially the same value as the viscosity average molecular weight of the ultra-high molecular weight polyethylene powder constituting the polyethylene resin composition.

[0125] The method for controlling the viscosity average molecular weight (Mv) of the polyethylene resin composition within the above range is not particularly limited, and examples thereof include a method of adjusting the polymerization temperature of a reactor when homopolymerizing ethylene or copolymerizing ethylene with an olefin copolymerizable with ethylene.

[0126] The higher the polymerization temperature, the lower the viscosity average molecular weight (Mv), and the lower the polymerization temperature, the higher the viscosity average molecular weight (Mv). In addition, other methods for adjusting the viscosity average molecular weight (Mv) to the above range are not particularly limited, and examples thereof include a method of appropriately selecting the type of an organic metal compound used as a co-catalyst when homopolymerizing ethylene or copolymerizing ethylene with an olefin copolymerizable with ethylene.

[0127] In addition, other methods for adjusting the viscosity average molecular weight (Mv) to the above range are not particularly limited, and examples thereof include a method of adding a chain transfer agent when homopolymerizing ethylene or when copolymerizing ethylene with an olefin copolymerizable with ethylene. By adding a chain transfer agent, there is a tendency that the viscosity average molecular weight of the generated ultrahigh molecular weight polyethylene powder is reduced even at the same polymerization temperature.

[0128] (Metallic Soap)

[0129] The polyethylene resin composition of the present embodiment contains a metal soap.

[0130] The content of the metal soap in the polyethylene resin composition of the present embodiment is preferably 0.01 mass % to 0.3 mass %, more preferably 0.05 mass % to 0.25 mass %, further preferably 0.1 mass % to 0.20 mass %.

[0131] By having a metal soap content of 0.01% by mass or more, the fluidity of the polyethylene resin composition can be improved, and hopper clogging can be suppressed. In addition, when the polyethylene resin composition is processed to form a diaphragm, the smoothness of the diaphragm can be improved. This is because, when assembling the battery, there is a process of winding the diaphragm and the electrode on a rod-shaped core. By improving the smoothness of the diaphragm, the core can be smoothly pulled out after the winding is completed, and the productivity is improved. In addition, it also has the effect of neutralizing the chlorine component from the catalyst residue used in the polymerization of ultra-high molecular weight polyethylene powder, which can prevent corrosion of the equipment.

[0132] In addition, by setting the content of metal soap to 0.3% by mass or less, the fracture strength of the diaphragm can be increased. This is because when the content of metal soap remaining in the diaphragm is high, the probability of remaining on the surface of the diaphragm increases, stress concentration occurs, and thus fracture occurs. By setting the content of metal soap to 0.3% by mass or less, the probability of remaining on the surface of the diaphragm is reduced, and fracture can be prevented.

[0133] (Twin-screw extrusion conditions)

[0134] When the polyethylene resin composition of the first embodiment is subjected to twin-screw extrusion under specific conditions, the aspect ratio of the strand deposit is Aspect Ratio = 0.05 or more and 7.0 or less.

[0135] When the polyethylene resin composition is subjected to twin-screw extrusion processing, a slurry obtained by mixing the polyethylene resin composition (ultra-high molecular weight polyethylene powder and metal soap) and liquid paraffin is used.

[0136] The amount of metal soap added during the twin-screw extrusion was 5% by mass of the ultra-high molecular weight polyethylene powder.

[0137] In addition, the polymer concentration is adjusted according to the viscosity average molecular weight (Mv) of the polyethylene resin composition. When the viscosity average molecular weight (Mv) is set to X and the polymer concentration is set to Y, the polymer concentration Y can be adjusted to be greater than the value of the following (Formula I) and less than the value of the following (Formula II), for example, adjusted to the polymer concentration (PC) shown in the following Table 1.

[0138] Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight (Mv)

[0139] Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight (Mv)

[0140] [Table 1]

[0141] Molecular weight (Mv) / ten thousand PC / weight% Molecular weight (Mv) / ten thousand PC / weight% Greater than or equal to 10 and less than 30 45 Greater than or equal to 150 and less than 200 15 Greater than or equal to 30 and less than 40 39 Greater than or equal to 200 and less than 300 12 Greater than or equal to 40 and less than 50 34 Greater than or equal to 300 and less than 400 10 Greater than or equal to 50 and less than 60 31 Greater than or equal to 400 and less than 500 9 Greater than or equal to 60 and less than 70 28 Greater than or equal to 500 and less than 600 8 Greater than or equal to 70 and less than 80 26 Greater than or equal to 600 and less than 700 7 Greater than or equal to 80 and less than 90 24 Greater than or equal to 700 and less than 800 6 Greater than or equal to 90 and less than 100 23 Greater than or equal to 800 and less than 900 6 Greater than or equal to 100 and less than 150 18 900 or more and 1000 or less 6

[0142] In addition, a counter-rotating twin-screw extruder is used as an extruder, the extrusion temperature is 160°C, the screw speed is 150rpm, the aperture of the discharge port is 1.0mm, the height from the discharge port to the ground is 1.0m or more and 1.1m or less, the discharge volume is 0.5kg / hour or more and 5.0kg / hour or less, the extrusion time is 1 hour, the atmosphere temperature and humidity are 15°C or more and 30°C or less, 20%RH or more and 70%RH or less, and the table material is aluminum. It should be noted that from the viewpoint of suppressing the deviation of the aspect ratio of the strand deposit, it is preferred to adjust the discharge volume to 2.0kg / hour or more and 3.0kg / hour or less, and more preferably to 2.5kg / hour. In addition, the discharge volume sometimes produces a change of ±0.5kg / hour relative to the set value.

[0143] (Aspect ratio of wire deposit)

[0144] The aspect ratio of the strand deposit extruded using the above-mentioned twin-screw extrusion conditions is calculated as follows: the maximum height of the deposit in the direction perpendicular to the ground is set as the longitudinal direction, the maximum spreading width in the direction horizontal to the ground is set as the transverse direction, and the longitudinal height is divided by the transverse spreading width.

[0145] Specifically, if Figure 1As shown in FIG. 1 , the polymer strands extruded under the above twin-screw extrusion conditions are piled up in a direction perpendicular to the ground. Next, the strands are cooled and solidified. When the strands are piled up in a direction perpendicular to the ground, the calculation is Figure 1 Next, the bottom cross section of the strand deposit is photographed, and based on the observed image, the equivalent circle diameter of the bottom cross section of the strand deposit is calculated using image analysis software and is taken as the length of W to calculate (H / W).

[0146] The aspect ratio (vertical / horizontal) of the strand deposit calculated in this manner is 0.05 to 7.0, preferably 0.05 to 5.0, more preferably 0.05 to 4.0, further preferably 0.07 to 3.0, particularly preferably 0.1 to 2.0.

[0147] When the aspect ratio of the strand deposit is 0.05 or more, the withstand voltage of the separator can be increased.

[0148] The bonding of the fatty acid and the metal in the metal soap has ionic bonding, and it also has conductivity even in an organic solvent. According to the type of metal and the length of the hydrocarbon chain of the fatty acid, the intensity of ionic bonding and covalent bonding changes, and the conductivity of the metal soap with strong covalent bonding decreases. This tendency is also shown in the result of dipole moment (polarity), and the metal soap with low conductivity has a tendency that the polarity also decreases. It can be considered that the charge that becomes the cause of the conductivity of the metal soap is located in the center of the micelle and is surrounded by hydrocarbon chains. According to the shape and size of the micelle, the mobility of the charge, i.e., the conductivity, is determined.

[0149] When the polarity of the metal soap is small, the conductivity of the polyethylene resin composition decreases and becomes easily charged. As a result, the strand deposits spread in the lateral direction and tend to become smaller (vertical / lateral).

[0150] On the other hand, when the polarity of the metal soap is high, the conductivity of the polyethylene resin composition increases and it is difficult to be charged. As a result, the strand deposits are deposited in the longitudinal direction and tend to be larger (longitudinal / lateral).

[0151] As can be seen from the above, the lower limit of the aspect ratio of the strand deposit of the polyethylene resin composition of the present embodiment is 0.05, which means that the conductivity of the metal soap is low, that is, the polarity difference with the ultra-high molecular weight polyethylene powder is small, and the dispersibility of the metal soap in the polyethylene resin composition of the present embodiment is good, so that even if the polyethylene resin composition is prepared, the conductivity is reduced, and as a result, the lower limit of the aspect ratio (vertical / horizontal) is 0.05. As a result, a separator that is not prone to short circuit can be obtained.

[0152] In addition, by setting the upper limit of the aspect ratio of the strand deposit to 7.0, the amount of deposits from the metal soap adhering to the extruder die lip can be suppressed. This is considered to be because the metal soap has low conductivity (small polarity of the metal soap), that is, the metal soap and liquid paraffin have good compatibility, so that the metal soap is difficult to seep out of the liquid paraffin, and as a result, the metal soap can be suppressed from spreading and adhering to the extruder die lip together with the liquid paraffin.

[0153] In addition, the quality of the diaphragm can be improved by adjusting the amount of metal soap remaining in the diaphragm to the minimum amount that can maintain the smoothness of the diaphragm. This is believed to be because the metal soap has good compatibility with liquid paraffin, and when the liquid paraffin is extracted from the film using an organic solvent (dichloromethane, hexane, etc.) after film formation, the metal soap is also extracted together with the liquid paraffin, thereby preventing the metal soap from remaining excessively in the film.

[0154] For the polyethylene resin composition of the present embodiment, there is no particular limitation on the method for controlling the aspect ratio of the strand deposit during twin-screw extrusion to be greater than 0.05 and less than 7.0, and an example thereof includes a method of adding a metal soap having low conductivity (good compatibility with liquid paraffin). As a method for reducing the conductivity of the metal soap, there are conceivable methods of adjusting the type of metal (the dipole moment decreases in the order of Ca>Mg>Zn) or a method of extending the hydrocarbon chain length of the fatty acid.

[0155] Specifically, the following method can be considered.

[0156] The first method is a method of adding methanol to the metal soap and then drying it. This method is a method in which alcohol (methanol, etc.) is sprayed into the metal soap produced by a dry method or a wet method, stirred, and then dried in a temperature range of -70°C to -20°C, the melting point of the metal soap. By adjusting in this way, the water in the metal soap is azeotroped with the alcohol, and the water and hydrates in the metal soap evaporate, thereby making the crystal structure denser and less likely to be dispersed in liquid paraffin. The amount of metal soap present in the state of micelles during extrusion increases, so the conductivity decreases.

[0157] The second method is a method of quenching the metal soap after the reaction. This method is as follows: when the metal soap is produced by a dry method or a wet method, it is quenched from a high temperature to room temperature after the reaction process is completed. The cooling rate needs to be adjusted to 0.5°C / min or more and 5.0°C / min or less. As a result, the crystal structure becomes dense, and it is not easy to disperse in liquid paraffin. The amount of metal soap present in the state of micelles during extrusion increases, so the conductivity decreases.

[0158] (Average number of carbon atoms per alkyl chain of metal soap)

[0159] In the first embodiment, the average number of carbon atoms per alkyl chain of the metal soap contained in the polyethylene resin composition of the present embodiment is preferably 16.0 to 28.0, more preferably 16.0 to 22.0, and even more preferably 16.0 to 20.0.

[0160] In the second embodiment, the average number of carbon atoms per alkyl chain of the metal soap contained in the polyethylene resin composition is 16.0 to 28.0, preferably 16.0 to 22.0, and more preferably 16.0 to 20.0.

[0161] When the average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more, the compatibility of the metal soap with the liquid paraffin is improved when the polymer and the metal soap are kneaded in the presence of liquid paraffin in the manufacturing process of the polyethylene resin composition, and the metal soap is not easily exuded from the liquid paraffin, resulting in the metal soap being prevented from adhering to the die lip of the extruder together with the liquid paraffin in the form of deposits. In addition, since the metal soap has low electrical conductivity, short circuit is not easily caused, and the withstand voltage of the diaphragm can be improved.

[0162] Furthermore, since the average number of carbon atoms per alkyl chain of the metal soap is 28.0 or less, the amount of metal soap remaining in the film can be minimized while maintaining the slipperiness of the film using the polyethylene resin composition of this embodiment, resulting in improved film quality.

[0163] As described in the method for producing a polyethylene resin composition described later, the average number of carbon atoms per alkyl chain of the metal soap can be adjusted to the above numerical range by appropriately selecting the fatty acid used in the production step of the metal soap.

[0164] The average number of carbon atoms per alkyl chain of the metal soap contained in the polyethylene resin composition of the present embodiment can be measured by the following method.

[0165] First, the metal soap is extracted from the polyethylene resin composition.

[0166] As the extraction method, two methods can be cited. The first method is a method using a mixed solvent of chloroform / propylene glycol (mass ratio: 9 / 1). The polyethylene resin composition is put into the mixed solvent, stirred at room temperature for 30 minutes to 1 hour, and then filtered. Methanol is added to the obtained solvent to reprecipitate it, and filtered again to obtain a metal soap.

[0167] In addition, in addition to the reprecipitation with methanol, there is also a method of obtaining a metal soap by removing the solvent under reduced pressure and heating using an evaporator while controlling the boiling point.

[0168] The second method is a method using a toluene solvent. The polyethylene resin composition is placed in a toluene solvent adjusted to 95°C or higher and 100°C or lower, stirred for 30 minutes to 1 hour, and then filtered. Methanol is added to the obtained solvent to reprecipitate, and filtered again to obtain a metal soap.

[0169] In addition, in addition to the reprecipitation with methanol, there is also a method of obtaining a metal soap by removing the solvent under reduced pressure and heating using an evaporator while controlling the boiling point.

[0170] Next, the extracted metal soap is analyzed using gas chromatography (GC), thereby being able to calculate the ratio of each hydrocarbon chain length and to determine the average number of carbon atoms per alkyl chain of the metal soap.

[0171] Weigh 100 mg of metal soap accurately and take it to a small conical flask equipped with a reflux condenser. Add 5.0 mL of boron trifluoride methanol reagent and shake well, and heat for about 10 minutes until dissolved. Add 4.0 mL of heptane from the condenser and heat for about 10 minutes. After cooling, add 20 mL of saturated sodium chloride solution and shake well, and let it stand to separate the liquid into two layers. The separated heptane layer is passed through about 0.1 g of anhydrous sodium sulfate that has been previously washed with heptane and taken to another flask. Take 1.0 mL of this liquid to a 10 mL volumetric flask, add heptane to make it accurately 10 mL and shake well to prepare a sample solution.

[0172] 1 μL of the sample solution was tested by gas chromatography under the following conditions. The peak area A of methyl stearate and the peak area B of all fatty acid esters obtained (total peak areas detected) of the sample solution were measured, and the ratio (%) of stearic acid in the fatty acid component of the metal soap was calculated according to the following formula.

[0173] Stearic acid ratio (%) = A / B × 100

[0174] Similarly, the ratio (%) of palmitic acid contained in the metal soap was calculated.

[0175] The peak area of ​​methyl stearate is more than 40% of the total area of ​​the peak of all fatty acid esters obtained by the chromatogram, and the total peak area of ​​methyl stearate and methyl palmitate is more than 90% of the total area of ​​the peak of all fatty acid esters obtained by the chromatogram. It should be noted that in the measurement solution, except stearic acid and palmitic acid, also contain some other higher fatty acids, therefore when the containing ratio of stearic acid and palmitic acid is tested by gas chromatography, the presence of other higher fatty acids is defined as below 10%.

[0176] Operating conditions

[0177] Detector: Hydrogen flame ionization detector maintained at approximately 260°C

[0178] Sample introduction: Splitless injection section maintained at approximately 220°C

[0179] Column: A column obtained by coating the inner surface of a quartz column having an inner diameter of about 0.32 mm and a length of about 30 m with polyethylene glycol 15000-diepoxide for gas chromatography at a thickness of 0.5 μm.

[0180] Column temperature: maintained at 70°C for about 2 minutes after the sample was injected, then increased to 240°C at a rate of 5°C per minute, and then maintained at this temperature for 5 minutes.

[0181] Carrier gas: Helium

[0182] Flow rate: Constant flow rate of about 50 cm per second

[0183] Selection of columns: The following columns were used: About 50 mg of stearic acid for gas chromatography and about 50 mg of palmitic acid for gas chromatography, which had been dried for 4 hours using a desiccant (silica gel), were accurately weighed and placed in a small conical flask equipped with a reflux condenser. 5.0 ml of boron trifluoride·methanol test solution was added and shaken well, and the following operation was performed in the same manner as the sample solution to prepare a device adjustment solution. When 1 μL of the liquid was operated under the above operating conditions, the relative retention time ratio of methyl palmitate to methyl stearate was about 0.86, and the resolution was 5.0 or more.

[0184] Reproducibility of the test: When the device adjustment solution was repeatedly tested 6 times under the above conditions, the relative standard deviation of the peak areas of methyl palmitate and methyl stearate was 6.0% or less. In addition, the relative standard deviation of the peak area ratio of methyl palmitate to methyl stearate obtained by the repeated test was 1.0% or less.

[0185] (C18 / C16 ratio of metal soap)

[0186] The metal soap used in the polyethylene resin composition of the present embodiment preferably contains a fatty acid having 16 carbon atoms per alkyl chain (C16) and a fatty acid having 18 carbon atoms per alkyl chain (C18), and their mass ratio C18 / C16 is preferably 1.5 to 1000, more preferably 1.5 to 900, and even more preferably 2.0 to 800.

[0187] When the mass ratio of metal soap C18 / C16 is 1.5 or more, the compatibility of metal soap and liquid paraffin is improved, and metal soap is not easy to ooze out of liquid paraffin, and as a result, it is possible to suppress the metal soap and liquid paraffin from adhering to the extruder die lip. In addition, the conductivity of the metal soap is reduced (easy to be charged), which can improve the durability of the diaphragm when a voltage is applied.

[0188] Furthermore, when the mass ratio C18 / C16 of the metal soap is 1000 or less, the amount of the metal soap remaining in the film can be minimized while maintaining the slipperiness of the film using the polyethylene resin composition of the present embodiment, resulting in improved film quality.

[0189] In addition, the C18 / C16 ratio of the metal soap can be measured by the method described in the Examples mentioned later.

[0190] As will be described later in the method for producing a polyethylene resin composition, the C18 / C16 ratio of the metal soap can be adjusted to fall within the above numerical range by appropriately selecting the fatty acid used in the production step of the metal soap.

[0191] (Ca ion concentration of metal soap)

[0192] The Ca ion concentration of the metal soap contained in the polyethylene resin composition of the present embodiment is preferably 1.0 mg / L to 200 mg / L, more preferably 1.0 mg / L to 180 mg / L, further preferably 1.0 mg / L to 100 mg / L, and still more preferably 1.0 mg / L to 50 mg / L.

[0193] By making the Ca ion concentration of the metal soap greater than 1.0 mg / L, it is possible to capture the catalyst residue (chlorine) contained in the ultra-high molecular weight polyethylene powder which is the raw material of the polyethylene resin composition of this embodiment, prevent the chlorine from reacting with water to form hydrochloric acid, thereby preventing the formation of rust (corrosion) in the extruder system.

[0194] In addition, by setting the Ca ion concentration of the metal soap to 200 mg / L or less, it is possible to prevent the Ca ions from reacting with water to form calcium hydroxide, which can prevent the separator from being clogged by the calcium hydroxide. As a result, it is possible to prevent the charge and discharge efficiency of the manufactured battery from being deteriorated.

[0195] In addition, the Ca ion concentration of a metal soap can be measured by the method described in the Example mentioned later.

[0196] The Ca ion concentration of the metal soap can be controlled within the above numerical range by adjusting the respective input amounts of the fatty acid and the metal when reacting the fatty acid and the metal and the washing step (time / number of times) of the metal soap with pure water.

[0197] (Fatty acid amount in metal soap)

[0198] The content of the fatty acid having 16 or 18 carbon atoms in the metal soap contained in the polyethylene resin composition of the present embodiment is preferably 0.1 mass % to 2.0 mass %, more preferably 0.1 mass % to 1.9 mass %, further preferably 0.1 mass % to 1.8 mass %, further more preferably 0.1 mass % to 1.5 mass %.

[0199] When the content of the fatty acid having 16 or 18 carbon atoms in the metal soap is 0.1 mass % or more, the metal soap is easily dispersed in the liquid paraffin, and the slipperiness of a film produced using the polyethylene resin composition of the present embodiment tends to be improved.

[0200] In addition, by setting the content of the fatty acid having 16 or 18 carbon atoms in the metal soap to 2.0 mass % or less, it is possible to prevent a part of the fatty acid from being thermally decomposed during film production to leave burn marks on the extruder die lip or adhere to the screen. As a result, the amount of scale generated can be suppressed, and the generation of striations (ribs) in the separator or an increase in film defects can be prevented.

[0201] The amount of the fatty acid having 16 or 18 carbon atoms in the metal soap can be measured by the method described in Examples below.

[0202] (Crystallinity of polyethylene resin composition)

[0203] The crystallinity of the polyethylene resin composition of the present embodiment is preferably 70% to 80%, more preferably 70% to 78%, and even more preferably 70% to 75%.

[0204] The polyethylene resin composition of the present embodiment tends to be able to provide a high-strength molded product when the crystallinity is 70% or more.

[0205] Furthermore, the polyethylene resin composition of the present embodiment tends to be easy to mold and process, and has excellent processability, because the crystallinity is 80% or less.

[0206] In the present embodiment, the method for controlling the crystallinity of the polyethylene resin composition within the above range is not particularly limited, and for example, a method of adjusting the drying temperature and the drying time may be considered. In the present embodiment, the crystallinity can be measured by the method described in the examples described below.

[0207] (Titanium Content and Aluminum Content in Polyethylene Resin Composition)

[0208] The titanium (Ti) content in the polyethylene resin composition of the present embodiment is preferably 0.1 ppm to 5.0 ppm, more preferably 0.5 ppm to 5.0 ppm, and even more preferably 1.0 ppm to 4.0 ppm.

[0209] The aluminum (Al) content in the polyethylene resin composition of the present embodiment is preferably 0.1 ppm to 5.0 ppm, more preferably 0.1 ppm to 4.0 ppm, and even more preferably 0.1 ppm to 3.5 ppm.

[0210] The polyethylene resin composition of this embodiment has a tendency to have better thermal stability and better long-term stability of the obtained molded product by adjusting the titanium content and the aluminum content within such a range. In addition, there is a tendency to suppress the reaction with the antioxidant or heat stabilizer added during processing and to suppress the coloring of the molded product caused by the generation of an organic metal complex.

[0211] Furthermore, the polyethylene resin composition of the present embodiment can obtain fibers having uniform diameters when made into fibers, and can obtain films having uniform thicknesses when made into films, by adjusting the titanium content and the aluminum content within the above ranges.

[0212] Generally, since the amount of metal derived from the catalyst residue remaining in the polyethylene resin composition is large, it tends to cause uneven thickness of the molded article.

[0213] It should be noted that the contents of Ti and Al in the polyethylene resin composition can be controlled by the productivity of the ethylene homopolymer or ethylene-based polymer per unit catalyst.

[0214] The productivity of ethylene homopolymer or ethylene polymer can be controlled by polymerization temperature, polymerization pressure, slurry concentration of the reactor when manufacturing. That is, in order to improve the productivity of the ethylene homopolymer or ethylene polymer used in the present embodiment, there is no particular restriction, for example, can enumerate and improve polymerization temperature, improve polymerization pressure and / or improve slurry concentration. As other methods, also can be by the selection of the kind of the co-catalyst component when obtaining ethylene homopolymer or ethylene polymer in polymerization, reduce the concentration of the co-catalyst component, utilize acid or alkali to clean ethylene homopolymer or ethylene polymer and control the aluminum amount.

[0215] In addition, in this embodiment, the content of Ti and Al can be measured by the method described in the examples mentioned later.

[0216] [Method for producing polyethylene resin composition]

[0217] The polyethylene resin composition of the present embodiment is obtained by producing an ultra-high molecular weight polyethylene powder, and adding and mixing a metal soap in the presence of liquid paraffin.

[0218] As a mixing method, for example, there can be mentioned a method of kneading using a Labo Plastomill (main body model: 4C150) manufactured by Toyo Seiki Co., Ltd. with a counter-rotating twin-screw extruder (main body model: 2D25S).

[0219] (Method for producing ultra-high molecular weight polyethylene powder)

[0220] <Catalyst ingredients>

[0221] The catalyst component used for producing the ultra-high molecular weight polyethylene powder used in the polyethylene resin composition of the present embodiment is not particularly limited, and examples thereof include common Ziegler-Natta catalysts.

[0222] [Ziegler-Natta catalyst]

[0223] The Ziegler-Natta catalyst is preferably a catalyst for olefin polymerization, which comprises a solid catalyst component [A] and an organometallic compound component [B], wherein the solid catalyst component [A] is produced by reacting an organomagnesium compound (A-1) soluble in an inert hydrocarbon solvent and represented by the following (Formula 1) with a titanium compound (A-2) represented by the following (Formula 2) using an inert hydrocarbon solvent.

[0224] (A-1): (M 1 ) α (Mg) β (R 2 ) a (R 3 ) b (Y 1 ) c ……(Formula 1)

[0225] (In Formula 1, M 1 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 2 and R 3 is a hydrocarbon group having 2 or more and 20 or less carbon atoms, Y 1 Alkoxy, silyloxy, allyloxy, amino, amide, -N=CR 4 ,R 5 、-SR 6 (Here, R 4 , R 5 and R 6 is a hydrocarbon group having 1 to 20 carbon atoms. 1α, β, a, b and c are real numbers satisfying the following relationship: 0≤α, 0<β, 0≤a, 0≤b, 0≤c, 0<a+b, 0≤c / (α+β)≤2, nα+2β=a+b+c (here, n represents M 1 valence.

[0226] (A-2): Ti(OR 7 ) d X 1 (4-d) ……(Formula 2)

[0227] (In Formula 2, d is a real number greater than or equal to 0 and less than or equal to 4, R 7 is a hydrocarbon group having 1 to 20 carbon atoms, X 1 is a halogen atom.)

[0228] It should be noted that examples of the inert hydrocarbon solvent used in the reaction of the organomagnesium compound (A-1) and the titanium compound (A-2) include, but are not limited to, aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane.

[0229] First, the organomagnesium compound (A-1) will be described.

[0230] The organomagnesium compound (A-1) is shown in the form of an organomagnesium complex soluble in an inert hydrocarbon solvent, including all dihydrocarbyl magnesium compounds and complexes of the compound with other metal compounds. The relationship between the symbols α, β, a, b, c is nα+2β=a+b+c, which represents the stoichiometry of the valence of the metal atom and the substituent.

[0231] In (Formula 1), as R 2 and R 3 The hydrocarbon group having 2 to 20 carbon atoms is, for example, an alkyl group, a cycloalkyl group or an aryl group, and specifically, ethyl group, propyl group, butyl group, pentyl group, hexyl group, octyl group, decyl group, cyclohexyl group, phenyl group and the like are mentioned, but not limited thereto. An alkyl group is particularly preferred.

[0232] In the case of α>0, as the metal atom M 1 A metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table can be used, and examples thereof include zinc, boron, aluminum, etc. Aluminum and zinc are particularly preferred.

[0233] For magnesium relative to metal atoms M 1The ratio β / α is not particularly limited, but is preferably 0.1 to 30, and more preferably 0.5 to 10. In the case of using a predetermined organomagnesium compound with α=0, for example, in R 2 In the case of 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferred result in the present embodiment.

[0234] In the above (Formula 1), it is recommended that R 2 , R 3 Satisfies any one of the following three groups: (1), (2), and (3).

[0235] Group (1): R 2 , R 3 At least one of them is a secondary or tertiary alkyl group having 4 or more and 6 or less carbon atoms, preferably R 2 , R 3 All are alkyl groups having 4 to 6 carbon atoms, and at least one is a secondary alkyl group or a tertiary alkyl group.

[0236] Group (2): R 2 and R 3 are alkyl groups with different carbon number, preferably R 2 is an alkyl group having 2 or 3 carbon atoms and R 3 It is an alkyl group having 4 or more carbon atoms.

[0237] Group (3): R 2 , R 3 At least one of them is a hydrocarbon group having 6 or more carbon atoms, and it is preferred that R 2 , R 3 The total number of carbon atoms contained in the alkyl group is 12 or more.

[0238] These groups are specifically shown below.

[0239] In the above group (1), examples of the secondary or tertiary alkyl group having 4 to 6 carbon atoms include 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl. 1-methylpropyl is particularly preferred.

[0240] In the above group (2), examples of the alkyl group having 2 or 3 carbon atoms include ethyl, 1-methylethyl, propyl, etc. Among them, ethyl is particularly preferred. In addition, there are no particular restrictions on the alkyl group having 4 or more carbon atoms, and specific examples include butyl, pentyl, hexyl, heptyl, octyl, etc. Butyl and hexyl are particularly preferred.

[0241] In the above group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, and examples thereof include hexyl, heptyl, octyl, nonyl, decyl, phenyl, 2-naphthyl, etc. Among the hydrocarbon groups, alkyl groups are preferred, and among the alkyl groups, hexyl and octyl groups are particularly preferred.

[0242] Generally, when the number of carbon atoms contained in the alkyl group increases, it tends to be easily dissolved in an inert hydrocarbon solvent, and also tends to have a tendency to increase the viscosity of the solution. Therefore, from an operational point of view, it is preferred to use a compound having an alkyl group with a moderately long chain. It should be noted that the above-mentioned organomagnesium compound can be used after being diluted with an inert hydrocarbon solvent, and can be used without problems even if a trace amount of Lewis basic compounds such as ether, ester, amine, etc. is contained or remains in the solution.

[0243] Next, for Y 1 Provide explanation.

[0244] In the above (Formula 1), Y 1 Alkoxy, silyloxy, allyloxy, amino, amide, -N=CR 4 ,R 5 、-SR 6 (Here, R 4 , R 5 and R 6 Each independently represents a hydrocarbon group having 1 to 20 carbon atoms), a β-keto acid residue.

[0245] In the above (Formula 1), as R 4 , R 5 and R 6 The hydrocarbon group represented by is 1 to 20 carbon atoms, preferably an alkyl group or an aryl group having 1 to 12 carbon atoms, and more preferably an alkyl group or an aryl group having 3 to 10 carbon atoms. For example, methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl, etc. can be cited, but there is no particular limitation. Butyl, 1-methylpropyl, 2-methylpentyl and 2-ethylhexyl are particularly preferred.

[0246] In addition, in the above (Formula 1), Y 1 Preferred is an alkoxy group or a siloxy group.

[0247] As the alkoxy group, for example, methoxy, ethoxy, propoxy, 1-methylethoxy, butoxy, 1-methylpropoxy, 1,1-dimethylethoxy, pentoxy, hexoxy, 2-methylpentoxy, 2-ethylbutoxy, 2-ethylpentoxy, 2-ethylhexyloxy, 2-ethyl-4-methylpentoxy, 2-propylheptyloxy, 2-ethyl-5-methyloctyloxy, octyloxy, phenoxy, naphthoxy, but not limited thereto. Particularly more preferred are butoxy, 1-methylpropoxy, 2-methylpentoxy and 2-ethylhexyloxy.

[0248] As the silyloxy group, for example, dimethylhydrogensilyloxy, ethylmethylhydrogensilyloxy, diethylhydrogensilyloxy, trimethylsilyloxy, ethyldimethylsilyloxy, diethylmethylsilyloxy, triethylsilyloxy, etc. are preferred, but not limited thereto. Particularly, dimethylhydrogensilyloxy, ethylmethylhydrogensilyloxy, diethylhydrogensilyloxy, trimethylsilyloxy are more preferred.

[0249] The method for synthesizing the organomagnesium compound (A-1) is not particularly limited, and can be synthesized, for example, by: reacting a molten magnesium compound represented by the formula R in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C. 2 MgX 1 Japanese R 2 Mg(R 2 For the above meaning, X 1 The organomagnesium compound of the group consisting of halogen) and the organomagnesium compound of the formula M 1 R 3 n and M 1 R 3 (n-1) H(M 1 and R 3 As mentioned above, n represents M 1 The organic metal compound of the group consisting of (a) and (b) is reacted, if necessary, with a 1 -H(Y 1 The compound represented by Y 1 wherein the organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an organomagnesium compound of formula Y 1 In the case of reacting a compound represented by -H, there is no particular limitation on the order of the reaction. For example, the organic magnesium compound can be added with a compound represented by formula Y 1 -H represented by the method of formula Y 1 -H represents a method of adding an organic magnesium compound to a compound of formula Y 1 Any of the two methods of preparing a compound represented by -H.

[0250] Y in the above-mentioned organomagnesium compound (A-1) 1 The molar composition ratio c / (α+β) relative to all metal atoms is 0≤c / (α+β)≤2, preferably 0≤c / (α+β)<1. 1 When the molar composition ratio relative to all metal atoms is 2 or less, the reactivity of the organomagnesium compound (A-1) with respect to the titanium compound (A-2) tends to be improved.

[0251] Next, the titanium compound (A-2) is described.

[0252] (A-2) is a titanium compound represented by (Formula 2).

[0253] (A-2): Ti(OR 7 ) d X 1 (4-d) ……(Formula 2)

[0254] (In Formula 2, d is a real number greater than or equal to 0 and less than or equal to 4, R 7 is a hydrocarbon group having 1 to 20 carbon atoms, X 1 is a halogen atom.)

[0255] In the above (Formula 2), d is preferably 0 or more and 1 or less, and more preferably 0.

[0256] In the above (Formula 2), R 7 Examples of the hydrocarbon group represented by include, but are not limited to, aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and allyl; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl; and aromatic hydrocarbon groups such as phenyl and naphthyl. Aliphatic hydrocarbon groups are particularly preferred.

[0257] As X 1 The halogen atom represented by may be, for example, chlorine, bromine, or iodine. Chlorine is particularly preferred. The titanium compound (A-2) is particularly preferably titanium tetrachloride. In this embodiment, two or more compounds selected from the above compounds may be mixed and used.

[0258] Next, the reaction between the organomagnesium compound (A-1) and the titanium compound (A-2) will be described.

[0259] The reaction is preferably carried out in an inert hydrocarbon solvent, more preferably in an aliphatic hydrocarbon solvent such as hexane or heptane. The molar ratio of the organomagnesium compound (A-1) to the titanium compound (A-2) in the reaction is not particularly limited, but the molar ratio (Ti / Mg) of the Ti atoms contained in the titanium compound (A-2) to the Mg atoms contained in the organomagnesium compound (A-1) is preferably 0.1 to 10, more preferably 0.3 to 3.

[0260] The reaction temperature is not particularly limited, but is preferably in the range of -80°C to 150°C, more preferably in the range of -40°C to 100°C.

[0261] The order of adding the organomagnesium compound (A-1) and the titanium compound (A-2) is not particularly limited, and the method may be any of adding the titanium compound (A-2) after the organomagnesium compound (A-1), adding the organomagnesium compound (A-1) after the titanium compound (A-2), and adding the organomagnesium compound (A-1) and the titanium compound (A-2) simultaneously, but the method of adding the organomagnesium compound (A-1) and the titanium compound (A-2) simultaneously is preferred. In the present embodiment, the solid catalyst component [A] obtained by the above reaction is used in the form of a slurry solution using an inert hydrocarbon solvent.

[0262] As other examples of the Ziegler-Natta catalyst component used in the present embodiment, the following olefin polymerization catalyst can be cited as a preferred example, wherein the olefin polymerization catalyst comprises a solid catalyst component [C] and an organic metal compound component [B], and the solid catalyst component [C] is produced by supporting an organic magnesium compound (C-4) soluble in an inert hydrocarbon solvent represented by the following (Formula 5) and a titanium compound (C-5) represented by the following (Formula 6) on a carrier (C-3) prepared by reacting an organic magnesium compound (C-1) soluble in an inert hydrocarbon solvent represented by the following (Formula 3) with a chlorinating agent (C-2) represented by the following (Formula 4).

[0263] (C-1): (M 2 ) γ (Mg) δ (R 8 ) e (R 9 ) f (OR 10 ) g ……(Formula 3)

[0264] (In Formula 3, M 2 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 8 , R 9 and R10 Each is a hydrocarbon group having 1 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers satisfying the following relationship: 0≤γ, 0<δ, 0≤e, 0≤f, 0≤g, 0<e+f, 0≤g / (γ+δ)≤2, kγ+2δ=e+f+g (here, k represents M 2 valence.

[0265] (C-2): H h SiCl i R 11 (4-(h+i)) ……(Formula 4)

[0266] (In Formula 4, R 11 is a hydrocarbon group having 1 or more and 12 or less carbon atoms, and h and i are real numbers satisfying the following relationship: 0<h, 0<i, 0<h+i≤4)

[0267] (C-4): (M 1 ) α (Mg) β (R 2 ) a (R 3 ) b Y 1 c ……(Formula 5)

[0268] (In Formula 5, M 1 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 2 and R 3 is a hydrocarbon group having 2 or more and 20 or less carbon atoms, Y 1 Alkoxy, silyloxy, allyloxy, amino, amide, -N=CR 4 ,R 5 、-SR 6 (Here, R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 α, β, a, b and c are real numbers satisfying the following relationship: 0≤α, 0<β, 0≤a, 0≤b, 0≤c, 0<a+b, 0≤c / (α+β)≤2, nα+2β=a+b+c (here, n represents M 1 valence.

[0269] (C-5): Ti(OR 7 ) d X 1 (4-d)……(Formula 6)

[0270] (In Formula 6, d is a real number greater than or equal to 0 and less than or equal to 4, R 7 is a hydrocarbon group having 1 to 20 carbon atoms, X 1 is a halogen atom.)

[0271] First, the organomagnesium compound (C-1) is described. The organomagnesium compound (C-1) is shown in the form of an organomagnesium complex soluble in an inert hydrocarbon solvent, including all of dihydrocarbyl magnesium compounds and complexes of the compound with other metal compounds. The relationship between the symbols γ, δ, e, f and g in Formula 3, kγ+2δ=e+f+g, represents the stoichiometry of the valence of the metal atom and the substituent.

[0272] In the above formula 3, regarding R 8 or R 9 The hydrocarbon group having 1 to 20 carbon atoms represented by is, for example, an alkyl group, a cycloalkyl group or an aryl group, and specifically, methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, phenyl, etc. can be cited, but it is not limited thereto. Among them, R is preferably 8 and R 9 Each is an alkyl group.

[0273] In the case of α>0, as the metal atom M 2 A metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table can be used, and examples thereof include zinc, boron, and aluminum, and aluminum and zinc are particularly preferred.

[0274] Magnesium relative to metal atoms M 2 The ratio δ / γ is not particularly limited, but is preferably 0.1 to 30, and more preferably 0.5 to 10. In addition, when a predetermined organomagnesium compound having γ=0 is used, for example, in R 8 In the case of 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferred result in the present embodiment.

[0275] In the above (Equation 3), it is recommended that R 8 , R 9 Satisfies any one of the following three groups: (1), (2), and (3).

[0276] Group (1): R 8 , R 9 At least one of them is a secondary or tertiary alkyl group having 4 or more and 6 or less carbon atoms, preferably R 8 , R 9 All are alkyl groups having 4 to 6 carbon atoms, and at least one is a secondary alkyl group or a tertiary alkyl group.

[0277] Group (2): R 8 and R 9 are alkyl groups with different carbon number, preferably R 8 is an alkyl group having 2 or 3 carbon atoms and R 9 It is an alkyl group having 4 or more carbon atoms.

[0278] Group (3): R 8 , R 9 At least one of them is a hydrocarbon group having 6 or more carbon atoms, preferably in R 8 , R 9 The total number of carbon atoms contained in the alkyl group is 12 or more.

[0279] These groups are specifically shown below.

[0280] In group (1), examples of the secondary or tertiary alkyl group having 4 to 6 carbon atoms include 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl. 1-methylpropyl is particularly preferred.

[0281] In group (2), examples of the alkyl group having 2 or 3 carbon atoms include ethyl, 1-methylethyl, and propyl. Ethyl is particularly preferred. In addition, there are no particular restrictions on the alkyl group having 4 or more carbon atoms, and examples thereof include butyl, pentyl, hexyl, heptyl, and octyl. Butyl and hexyl are particularly preferred.

[0282] In group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, and examples thereof include hexyl, heptyl, octyl, nonyl, decyl, phenyl, 2-naphthyl, etc. Among the hydrocarbon groups, alkyl groups are preferred, and among the alkyl groups, hexyl and octyl groups are particularly preferred.

[0283] Generally, when the number of carbon atoms contained in the alkyl group increases, it tends to be easily dissolved in an inert hydrocarbon solvent and the viscosity of the solution tends to increase. Therefore, from an operational point of view, it is preferred to use a compound having an alkyl group with a moderately long chain. It should be noted that the above-mentioned organomagnesium compound is used in the form of an inert hydrocarbon solution, and can be used without problem even if a trace amount of Lewis basic compounds such as ethers, esters, and amines are contained or remain in the solution.

[0284] Next, the alkoxy group (OR 10 ) for explanation.

[0285] As R 10The hydrocarbon group represented by is 1 to 20 carbon atoms, preferably an alkyl group or aryl group having 1 to 12 carbon atoms, and particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. 10 , for example, methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl, etc., but not limited thereto. Particularly preferred are butyl, 1-methylpropyl, 2-methylpentyl and 2-ethylhexyl.

[0286] The method for synthesizing the organomagnesium compound (C-1) is not particularly limited, and the following method may be mentioned: in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C., a 8 MgX 1 Japanese R 8 Mg(R 8 For the above meaning, X 1 The organomagnesium compound of the group consisting of halogen atoms and the organic magnesium compound of the formula M 2 R 9 k Japanese M 2 R 9 (k-1) H(M 2 , R 9 and k has the above meanings) and then, if necessary, reacted with an organometallic compound having R 9 (R 9 The above meaning) represents a hydrocarbon alcohol or a hydrocarbon soluble in an inert hydrocarbon solvent having R 9 The alkoxymagnesium compound and / or alkoxyaluminum compound having a hydrocarbon group represented by is reacted.

[0287] When an organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an alcohol, the order of the reactions is not particularly limited, and any of a method of adding alcohol to the organomagnesium compound, a method of adding the organomagnesium compound to the alcohol, or a method of simultaneously adding both the organomagnesium compound and the alcohol can be used.

[0288] There is no particular restriction on the reaction ratio of the organic magnesium compound soluble in an inert hydrocarbon solvent and the alcohol. As a result of the reaction, the molar composition ratio of the alkoxy groups in the obtained organic magnesium compound containing alkoxy groups to all metal atoms, g / (γ+δ), is 0≤g / (γ+δ)≤2, preferably 0≤g / (γ+δ)<1.

[0289] Next, the chlorinating agent (C-2) is described. The chlorinating agent (C-2) is a chlorinated silicon compound having at least one Si-H bond represented by the following (Formula 4).

[0290] (C-2): H h SiCl i R 11 (4-(h+i)) ……(Formula 4)

[0291] (In Formula 4, R 11 is a hydrocarbon group having 1 or more and 12 or less carbon atoms, and h and i are real numbers satisfying the following relationship: 0<h, 0<i, 0<h+i≤4)

[0292] In the above (Formula 4), regarding R 11 The hydrocarbon group represented by is, for example, an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, and specifically, methyl, ethyl, propyl, 1-methylethyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, phenyl, etc., but not limited thereto. Among them, an alkyl group having 1 to 10 carbon atoms is preferred, and an alkyl group having 1 to 3 carbon atoms, such as methyl, ethyl, propyl, 1-methylethyl, is more preferred. In addition, h and i are numbers greater than 0 that satisfy the relationship of h+i≤4, and i is preferably 2 to 3.

[0293] Examples of the chlorinating agent (C-2) compound represented by (Formula 4) include: HSiCl3, HSiCl2CH3, HSiCl2C2H5, HSiCl2(C3H7), HSiCl2(2-C3H7), HSiCl2(C4H9), HSiCl2(C6H5), HSiCl2(4-Cl-C6H4), HSiCl2(CH=CH2), HSiCl2(CH2C6H5), HSiCl2(1-C 10 H7), HSiCl2(CH2CH=CH2), H2SiCl(CH3), H2SiCl(C2H5), HSiCl(CH3)2, HSiCl(C2H5)2, HSiCl(CH3)(2-C3H7), HSiCl(CH3)(C6H5), HSiCl(C6H5)2, etc., but not limited thereto. Use these compounds or chlorinated silicon compounds containing a mixture of two or more selected from these compounds. Among them, HSiCl3, HSiCl2CH3, HSiCl(CH3)2, HSiCl2(C3H7) are preferred, and HSiCl3 and HSiCl2CH3 are more preferred.

[0294] Next, the reaction of the above-mentioned organomagnesium compound (C-1) and the chlorinating agent (C-2) is described. During the reaction, it is preferred to use an inert hydrocarbon solvent, chlorinated hydrocarbons such as 1,2-dichloroethane, o-dichlorobenzene, and dichloromethane; an ether medium such as ether and tetrahydrofuran; or a mixed medium thereof to dilute the chlorinating agent (C-2) before use. Among them, inert hydrocarbon solvents are more preferred from the perspective of catalyst performance.

[0295] The reaction ratio of the organomagnesium compound (C-1) and the chlorinating agent (C-2) is not particularly limited, but the amount of silicon atoms contained in the chlorinating agent (C-2) is preferably 0.01 mol or more and 100 mol or less, and more preferably 0.1 mol or more and 10 mol or less, per 1 mol of magnesium atoms contained in the organomagnesium compound (C-1).

[0296] The reaction method of the organomagnesium compound (C-1) and the chlorinating agent (C-2) is not particularly limited, and any of the following methods can be used: a method of introducing the organomagnesium compound (C-1) and the chlorinating agent (C-2) into a reactor simultaneously and reacting them, a method of introducing the organomagnesium compound (C-1) into the reactor beforehand, or a method of introducing the organomagnesium compound (C-1) into the reactor beforehand and then introducing the chlorinating agent (C-2) into the reactor. Among them, the method of introducing the organomagnesium compound (C-1) into the reactor beforehand is preferred. The carrier (C-3) obtained by the above reaction is preferably separated by filtration or decantation, and then fully washed with an inert hydrocarbon solvent to remove unreacted substances or by-products.

[0297] The reaction temperature of the organomagnesium compound (C-1) and the chlorinating agent (C-2) is not particularly limited, but is preferably 25°C to 150°C, more preferably 30°C to 120°C, and further preferably 40°C to 100°C.

[0298] In the method of simultaneous addition in which the organomagnesium compound (C-1) and the chlorinating agent (C-2) are simultaneously introduced into a reactor and reacted, it is preferred that the temperature of the reactor is adjusted to a predetermined temperature in advance, and the temperature in the reactor is adjusted to maintain the predetermined temperature while the simultaneous addition is performed, thereby adjusting the reaction temperature to the predetermined temperature. In the method of previously introducing the chlorinating agent (C-2) into the reactor and then introducing the organomagnesium compound (C-1) into the reactor, it is preferred that the temperature of the reactor after the chlorinating agent (C-2) is introduced is adjusted to a predetermined temperature in advance, and the temperature in the reactor is adjusted to maintain the predetermined temperature while the organomagnesium compound (C-1) is introduced into the reactor, thereby adjusting the reaction temperature to the predetermined temperature. In the method of previously introducing the organomagnesium compound (C-1) into the reactor and then introducing the chlorinating agent (C-2) into the reactor, it is preferred that the temperature of the reactor after the organomagnesium compound (C-1) is introduced is adjusted to a predetermined temperature in advance, and the temperature in the reactor is adjusted to maintain the predetermined temperature while the chlorinating agent (C-2) is introduced into the reactor, thereby adjusting the reaction temperature to the predetermined temperature.

[0299] Next, the organomagnesium compound (C-4) is described. (C-4) is a compound represented by the above (Formula 5).

[0300] (C-4): (M 1 ) α (Mg) β (R 2 ) a (R 3 ) b Y 1 c ……(Formula 5)

[0301] (In Formula 5, M 1 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 2 and R 3 is a hydrocarbon group having 2 or more and 20 or less carbon atoms, Y 1 Alkoxy, silyloxy, allyloxy, amino, amide, -N=CR 4 ,R 5 、-SR 6 (Here, R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1α, β, a, b and c are real numbers satisfying the following relationship: 0≤α, 0<β, 0≤a, 0≤b, 0<a+b, 0≤c / (α+β)≤2, nα+2β=a+b+c (here, n represents M 1 valence.

[0302] The amount of the organomagnesium compound (C-4) used is preferably 0.1 to 10, more preferably 0.5 to 5, in terms of the molar ratio (Mg / Ti) of the magnesium atoms contained in the organomagnesium compound (C-4) to the titanium atoms contained in the titanium compound (C-5).

[0303] The reaction temperature of the organomagnesium compound (C-4) and the titanium compound (C-5) is not particularly limited, but is preferably in the range of -80°C to 150°C, more preferably in the range of -40°C to 100°C.

[0304] The concentration of the organomagnesium compound (C-4) when used is not particularly limited, but is preferably 0.1 mol / L to 2 mol / L, more preferably 0.5 mol / L to 1.5 mol / L, based on the magnesium atom contained in the organomagnesium compound (C-4). It should be noted that an inert hydrocarbon solvent is preferably used for diluting the organomagnesium compound (C-4).

[0305] There is no particular restriction on the order of adding the organomagnesium compound (C-4) and the titanium compound (C-5) to the carrier (C-3). The method may be any one of adding the titanium compound (C-5) after the organomagnesium compound (C-4), adding the organomagnesium compound (C-4) after the titanium compound (C-5), and adding the organomagnesium compound (C-4) and the titanium compound (C-5) simultaneously. Among them, the method of adding the organomagnesium compound (C-4) and the titanium compound (C-5) simultaneously is preferred. The reaction of the organomagnesium compound (C-4) and the titanium compound (C-5) is carried out in an inert hydrocarbon solvent, preferably an aliphatic hydrocarbon solvent such as hexane or heptane.

[0306] The catalyst obtained in the above manner is used in the form of a slurry solution using an inert hydrocarbon solvent.

[0307] Next, the titanium compound (C-5) is described. In the present embodiment, (C-5) is a titanium compound represented by the above (Formula 6).

[0308] (C-5): Ti(OR 7 ) d X 1 (4-d) ……(Formula 6)

[0309] (In Formula 6, d is a real number greater than or equal to 0 and less than or equal to 4, R 7 is a hydrocarbon group having 1 to 20 carbon atoms, X 1 is a halogen atom.)

[0310] In the above (Formula 6), as R 7 The hydrocarbon group represented by X may be, for example, aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and allyl; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl; and aromatic hydrocarbon groups such as phenyl and naphthyl, but is not limited thereto. Among them, aliphatic hydrocarbon groups are preferred. 1 The halogen represented by may be, for example, chlorine, bromine, and iodine, but is not limited thereto. Among them, chlorine is preferred. The titanium compound (C-5) selected from the above compounds may be used alone or in combination of two or more.

[0311] The amount of the titanium compound (C-5) used is not particularly limited, but is preferably 0.01 to 20, more preferably 0.05 to 10, in terms of molar ratio relative to the magnesium atoms contained in the support (C-3).

[0312] The reaction temperature of the organomagnesium compound (C-4) and the titanium compound (C-5) is not particularly limited, but is preferably in the range of -80°C to 150°C, more preferably in the range of -40°C to 100°C.

[0313] In the present embodiment, there is no particular limitation on the method for loading the titanium compound (C-5) on the carrier (C-3). A method of reacting an excess amount of the titanium compound (C-5) relative to the carrier (C-3), a method of effectively loading the titanium compound (C-5) by using a third component, and preferably a method of loading the titanium compound (C-5) by reacting the titanium compound (C-5) with an organic magnesium compound (C-4) can be used.

[0314] Next, the organometallic compound component [B] used in the present embodiment will be described.

[0315] The solid catalyst component for producing the ultra-high molecular weight polyethylene powder is a highly active polymerization catalyst obtained by combining the above-mentioned solid catalyst component [A] with an organometallic compound component [B]. The organometallic compound component [B] is sometimes also referred to as a "co-catalyst". The organometallic compound component [B] is preferably a compound containing a metal belonging to the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, and is particularly preferably an organoaluminum compound and / or an organomagnesium compound.

[0316] As the organoaluminum compound used as the organometallic compound component [B], it is preferred to use a compound represented by the following (Formula 7) alone or in combination.

[0317] AHr 12 j Z 1 (3-j) ……(Formula 7)

[0318] (In Formula 7, R 12 is a hydrocarbon group having 1 to 20 carbon atoms, Z 1 is a group belonging to the group consisting of hydrogen, halogen, alkoxy, allyloxy, and siloxy, and j is a number of 2 to 3.)

[0319] In the above (Formula 7), R 12 The hydrocarbon group having 1 or more and 20 or less carbon atoms includes aliphatic hydrocarbon groups, aromatic hydrocarbon groups, and alicyclic hydrocarbon groups, for example, preferably trialkylaluminum such as trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, tri(2-methylpropyl)aluminum (or triisobutylaluminum), tripentylaluminum, tri(3-methylbutyl)aluminum, trihexylaluminum, trioctylaluminum, and tridecylaluminum; aluminum halide compounds such as diethylaluminum chloride, ethylaluminum dichloride, bis(2-methylpropyl)aluminum chloride, ethylaluminum sesquichloride, and diethylaluminum bromide; alkoxyaluminum compounds such as ethoxydiethylaluminum and butoxybis(2-methylpropyl)aluminum; siloxyaluminum compounds such as dimethylhydrogensilyloxydimethylaluminum, ethylmethylhydrogensilyloxydiethylaluminum, and ethyldimethylsilyloxydiethylaluminum; and mixtures thereof, but not limited thereto. Particularly preferred are trialkylaluminum compounds.

[0320] As the organomagnesium compound used as the organometallic compound component [B], an organomagnesium compound soluble in an inert hydrocarbon solvent represented by the aforementioned (Formula 3) is preferred.

[0321] (M 2 ) γ (Mg) δ (R 8 ) e (R 9 ) f (OR 10 ) g ……(Formula 3)

[0322] (In Formula 3, M 2 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 8 , R 9 and R 10Each is a hydrocarbon group having 2 or more and 20 or less carbon atoms, and γ, δ, e, f, and g are real numbers satisfying the following relationship: 0≤γ, 0<δ, 0≤e, 0≤f, 0≤g, 0<e+f, 0≤g / (γ+δ)≤2, kγ+2δ=e+f+g (here, k represents M 2 valence.

[0323] The organomagnesium compound is shown in the form of an organomagnesium complex soluble in an inert hydrocarbon solvent, including all dihydrocarbylmagnesium compounds and complexes of the dihydrocarbylmagnesium compound and other metal compounds. 2 , R 8 , R 9 , OR 10 As already explained, since the solubility of the organomagnesium compound in the inert hydrocarbon solvent is preferably higher, δ / γ is preferably within the range of 0.5 or more and 10 or less, and more preferably M 2 Aluminum compounds.

[0324] The combination ratio of the solid catalyst component [A] and the organometallic compound component [B] is not particularly limited, but the organometallic compound component [B] is preferably 1 mmol or more and 3,000 mmol or less per 1 g of the solid catalyst component [A].

[0325] <Polymerization conditions of ultra-high molecular weight polyethylene powder>

[0326] The polymerization temperature in the method for producing the ultra-high molecular weight polyethylene powder as a raw material of the polyethylene resin composition of the present embodiment is usually 30° C. or higher and 100° C. or lower.

[0327] When the polymerization temperature is 30° C. or higher, more efficient production tends to be possible industrially. On the other hand, when the polymerization temperature is 100° C. or lower, more stable operation tends to be possible continuously.

[0328] The polymerization pressure in the method for producing the ultra-high molecular weight polyethylene powder used for the polyethylene resin composition of the present embodiment is usually not less than normal pressure and not more than 2 MPa.

[0329] The polymerization pressure is preferably 0.1 MPa or more, more preferably 0.12 MPa or more, and is preferably 1.5 MPa or less, more preferably 1.0 MPa or less.

[0330] When the polymerization pressure is above normal pressure, there is a tendency that more efficient production can be achieved industrially, and when the polymerization pressure is below 2 MPa, local heat generation caused by a rapid polymerization reaction when the catalyst is introduced can be suppressed, and there is a tendency that polyethylene can be produced stably.

[0331] The polymerization reaction may be carried out in any of a batch method, a semi-continuous method and a continuous method, but it is preferably carried out in a continuous method.

[0332] By continuously supplying ethylene gas, solvent, catalyst, etc. into the polymerization system, and continuously discharging with the generated polyethylene, the local high temperature state caused by the rapid reaction of ethylene can be suppressed, and the polymerization system is more stable. When ethylene reacts in a uniform state in the system, it is possible to suppress the generation of side chains, double bonds, etc. in the polymer chain, and it is not easy to produce low molecular weight polyethylene, crosslinking, so the residual unmelted material is reduced when the ultra-high molecular weight polyethylene powder is melted or melted, and coloring can be suppressed, and it is also not easy to produce problems such as mechanical properties reduction. Therefore, it is preferred that the polymerization system becomes more uniform in a continuous manner.

[0333] In addition, the polymerization of the ultrahigh molecular weight polyethylene powder can be carried out in two or more stages with different reaction conditions. In addition, the intrinsic viscosity of the obtained polyethylene powder can be adjusted by allowing hydrogen to exist in the polymerization system or by changing the polymerization temperature, as described in the specification of German Patent Application Publication No. 3127133.

[0334] By adding hydrogen as a chain transfer agent into the polymerization system, the intrinsic viscosity of the polyethylene powder can be controlled within an appropriate range.

[0335] When hydrogen is added to the polymerization system, the molar fraction of hydrogen is preferably 0 mol% to 30 mol%, more preferably 0 mol% to 25 mol%, and even more preferably 0 mol% to 20 mol%.

[0336] In addition, in the polymerization step, in addition to the above-mentioned components, other known components useful for the production of polyethylene may be contained.

[0337] When the ultra-high molecular weight polyethylene powder as the raw material of the polyethylene resin composition of the present embodiment is obtained by polymerization, in order to suppress the polymer from adhering to the polymerization reactor, an antistatic agent such as Stadis450 manufactured by The Associated Octel Company (agent Maruwa Bussan) can be used. Stadis450 can be added to the polymerization reactor by a pump or the like after being diluted in an inert hydrocarbon medium. Relative to the production of polyethylene per unit time, the addition amount at this time is preferably in the range of more than 0.10ppm and less than 20ppm, more preferably in the range of more than 0.20ppm and less than 10ppm.

[0338] <Additives>

[0339] To the ultra-high molecular weight polyethylene powder constituting the polyethylene resin composition of the present embodiment, additives such as a lubricant, a neutralizer, an antioxidant, a light stabilizer, an antistatic agent, and a pigment may be added as needed.

[0340] Examples of lubricants or neutralizers include, but are not limited to, aliphatic hydrocarbons, higher fatty acids, higher fatty acid metal salts, alcohol fatty acid esters, waxes, higher fatty acid amides, silicone oils, rosin, etc. The content of the lubricant or neutralizer is not particularly limited, but is generally 5000 ppm or less, preferably 4000 ppm or less, and more preferably 3500 ppm or less.

[0341] The antioxidant is not particularly limited, but phenolic compounds and phenolic phosphorus-containing compounds are preferred.

[0342] As antioxidants, for example, phenolic antioxidants such as 2,6-di-tert-butyl-4-methylphenol (butylhydroxytoluene), 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate, and tetrakis(methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate))methane; phenolic phosphorus-containing antioxidants such as 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine; and phosphorus-containing antioxidants such as 4,4'-biphenylene diphosphite tetrakis(2,4-di-tert-butylphenyl) ester, tris(2,4-di-tert-butylphenyl) phosphite, and cyclic neopentane tetraylbis(2,4-tert-butylphenyl phosphite), but are not limited thereto.

[0343] In the case where the polyethylene resin composition of the present embodiment includes ultra-high molecular weight polyethylene powder and liquid paraffin, when the total amount of the ultra-high molecular weight polyethylene powder and the liquid paraffin is 100 parts by mass, the amount of the antioxidant added is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, further preferably 3 parts by mass or less, and further more preferably 2 parts by mass or less. When the amount of the antioxidant is 5 parts by mass or less, the deterioration of the polyethylene powder can be suppressed, so that embrittlement, discoloration, reduction in mechanical properties, etc. are not likely to occur, and the long-term stability is more excellent.

[0344] Examples of the light stabilizer include benzotriazole-based light stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino)hexamethylene}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}], but are not limited thereto.

[0345] The content of the light-resistant stabilizer is not particularly limited, but is usually 5000 ppm or less, preferably 3000 ppm or less, and more preferably 2000 ppm or less.

[0346] Examples of the antistatic agent include, but are not limited to, aluminosilicate, kaolin, clay, natural silica, synthetic silica, silicates, talc, diatomaceous earth, and fatty acid glycerides.

[0347] (Method for producing metal soap)

[0348] The metal soap can be produced using higher fatty acids, polyvalent metal oxides or hydroxides, higher fatty acid metal salts, and the like.

[0349] <Raw materials>

[0350] As the higher fatty acid, a fatty acid having a carbon number of 16 or more and 28 or less can be used, such as palmitic acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid or a mixture thereof. These fatty acids can be mixed fatty acids like tallow fatty acid and palm oil fatty acid. Stearic acid and behenic acid are particularly preferred.

[0351] Examples of the oxide or hydroxide of the polyvalent metal include oxides or hydroxides of magnesium, calcium, strontium, barium, zinc, cadmium, lead, lithium, aluminum, copper, iron, cobalt and the like.

[0352] Examples of the higher fatty acid metal salt include lithium palmitate, sodium palmitate, magnesium palmitate, calcium palmitate, strontium palmitate, barium palmitate, zinc palmitate, aluminum palmitate, copper palmitate, lead palmitate, lithium stearate, sodium stearate, magnesium stearate, calcium stearate, strontium stearate, barium stearate, zinc stearate, aluminum stearate, copper stearate, lead stearate, lithium arachidate, sodium arachidate, magnesium arachidate, calcium arachidate, strontium palmitate, barium arachidate, zinc arachidate, aluminum arachidate, copper arachidate, lead arachidate, lithium behenate, sodium behenate, magnesium arachidate, calcium arachidate, strontium palmitate, barium arachidate, zinc arachidate, aluminum arachidate, copper arachidate, lead arachidate, lithium behenate, sodium behenate, Magnesium behenate, calcium behenate, strontium behenate, barium behenate, zinc behenate, aluminum behenate, copper behenate, lead behenate, lithium lignocerate, sodium lignocerate, magnesium lignocerate, calcium lignocerate, strontium lignocerate, barium lignocerate, zinc lignocerate, aluminum lignocerate, copper lignocerate, lead lignocerate, lithium lignocerate, sodium lignocerate, magnesium lignocerate, calcium lignocerate, strontium lignocerate, barium lignocerate, zinc lignocerate, aluminum lignocerate, copper lignocerate, lead lignocerate, lithium lignocerate, sodium lignocerate, magnesium lignocerate, calcium lignocerate, strontium lignocerate, barium lignocerate, zinc lignocerate, aluminum lignocerate, copper lignocerate, lead lignocerate, lithium lignocerate, sodium lignocerate, magnesium lignocerate, calcium lignocerate, strontium lignocerate, barium lignocerate, zinc lignocerate, aluminum lignocerate, copper lignocerate, lead lignocerate, etc.

[0353] From the viewpoint of molding processability (suppression of the amount of plateout etc.) and melt stability, magnesium stearate, calcium stearate, zinc stearate, magnesium behenate, calcium behenate and zinc behenate are particularly preferred.

[0354] <Production method>

[0355] It should be noted that as a method for preparing the metal soap used in the polyethylene resin composition of the present embodiment, there can be cited a method of treating a metal soap produced by a conventionally known industrial production method such as a wet method, a dry method, a double decomposition method, etc. (for example, a method for producing a metal soap described in Japanese Patent Application Laid-Open No. 11-35518) as follows.

[0356] The first method is a method of adding methanol to the metal soap and then drying it. This method is a method in which alcohol (methanol, etc.) is sprayed onto the metal soap produced by a dry method or a wet method, stirred, and then dried at a temperature ranging from -70°C to -20°C, the melting point of the metal soap. By performing such a treatment, the water in the metal soap is azeotroped with the alcohol, and the water and hydrates in the metal soap evaporate, thereby making the crystal structure denser and less likely to be dispersed in the liquid paraffin. The amount of metal soap present in the form of micelles during extrusion increases, and thus the conductivity decreases.

[0357] The second method is a method of quenching the metal soap after the reaction. This method is as follows: when the metal soap is produced by a dry method or a wet method, it is quenched from a high temperature to room temperature after the reaction process is completed. The cooling rate needs to be adjusted to 0.5°C / min or more and 5.0°C / min or less. As a result, the crystal structure becomes dense and difficult to disperse in liquid paraffin, and the amount of metal soap present in the state of micelles during extrusion increases, so the conductivity decreases.

[0358] [Molding body]

[0359] The molded article of the present embodiment is a molded article of the polyethylene resin composition of the first embodiment and the polyethylene resin composition of the second embodiment.

[0360] The molded article of the present embodiment can be obtained by molding the polyethylene resin composition of the first embodiment and the polyethylene resin composition of the second embodiment by various methods.

[0361] (Application of Molded Article)

[0362] The molded product of this embodiment can be used for various purposes.

[0363] The molded product of this embodiment is not limited, and is suitable as, for example, a microporous membrane, particularly a microporous membrane for secondary battery separators, particularly a microporous membrane for lithium ion secondary battery separators, a sintered body, a high-strength fiber, and the like.

[0364] The method for producing the microporous membrane is not particularly limited, and examples thereof include a processing method of extruding, stretching, extracting, and drying using an extruder equipped with a T-die in a wet process using a solvent.

[0365] Furthermore, the excellent characteristics of high molecular weight ethylene polymers, such as wear resistance, high sliding properties, high strength, and high impact resistance, can be utilized for a molded body (sintered body) obtained by sintering the polyethylene resin composition.

[0366] The method for producing the high-strength fiber is not particularly limited, and an example thereof includes a method of kneading liquid paraffin and the polyethylene resin composition, spinning the mixture, and then heating and stretching the mixture to obtain the high-strength fiber.

[0367] [Example]

[0368] Hereinafter, the present embodiment will be described in more detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples at all.

[0369] Ethylene and hexane used in Examples and Comparative Examples were dehydrated using MS-3A (manufactured by Showa Union Co., Ltd.), and hexane was used after being deoxygenated by further degassing under reduced pressure using a vacuum pump.

[0370] [Measurement method and conditions]

[0371] The physical properties of the polyethylene resin compositions of Examples and Comparative Examples were measured by the following methods.

[0372] ((1) Viscosity average molecular weight (Mv))

[0373] The viscosity average molecular weight Mv of the polyethylene resin compositions obtained in Examples and Comparative Examples was determined by the method shown below in accordance with ISO 1628-3 (2010).

[0374] First, 20 mg of a polyethylene resin composition was weighed in a dissolving tube, and the dissolving tube was purged with nitrogen. Then, 20 mL of decalin (decalin to which 1 g / L of 2,6-di-tert-butyl-4-methylphenol was added) was added, and the mixture was stirred at 150° C. for 2 hours to dissolve the polyethylene resin composition.

[0375] The falling time (ts) between the marked lines of the solution was measured using a Cannon-Fenske viscometer (manufactured by Shibata Scientific Instruments Co., Ltd.: product model-100) in a thermostatic bath at 135°C.

[0376] The falling time (ts) between the marked lines was measured in the same manner for samples in which the amount of the polyethylene resin composition was changed to 10 mg, 5 mg, and 2 mg.

[0377] As a blank, the falling time (tb) of decalin alone without adding the polyethylene resin composition was measured.

[0378] The reduced viscosity (ηsp / C) of the polyethylene resin composition was determined according to the following formula.

[0379] ηsp / C=(ts / tb-1) / 0.1(unit: dL / g)

[0380] The relationship between the concentration (C) (unit: g / dL) and the reduced viscosity (ηsp / C) of the polyethylene resin composition was plotted, and a linear approximation formula was derived by the least squares method and extrapolated to a concentration of 0 to determine the intrinsic viscosity ([η]).

[0381] Next, the viscosity average molecular weight (Mv) is calculated from the value of the intrinsic viscosity [η] using the following (Mathematical Formula A).

[0382] Mv=(5.34×10 4 )×[η] 1.49 (Mathematical formula A)

[0383] ((2) Metal Soap Content in Polyethylene Resin Composition (Mass %))

[0384] The metal soap content in the polyethylene resin composition obtained in Examples and Comparative Examples was determined by the method shown below.

[0385] When the measurement sample is irradiated with strong primary X-rays generated from an X-ray tube, the contained elements are excited and characteristic X-rays unique to the elements are generated. By introducing the X-rays into a spectroscopic chamber and analyzing the wavelength, the presence of the contained elements can be known. In addition, the content of the element can be obtained from the intensity of the characteristic X-rays, and the concentration of the additive in the polyethylene resin composition can be calculated from the content of the element.

[0386] First, a method for preparing a measurement sample is described below.

[0387] <Sample preparation: Preparation of a pressed sheet with a thickness of 3.0 mm>

[0388] The polyethylene resin composition was hot-pressed at 180°C / 1 MPa / 3 minutes and 180°C / 10 MPa / 2 minutes, and cold-pressed at 25°C / 10 MPa / 5 minutes to prepare a pressed sheet as a measurement sample.

[0389] It should be noted that the mold thickness used was 3.0 mm.

[0390] <Measurement of Additive Concentration in Polyethylene Resin Composition>

[0391] The produced pressed sheet is irradiated with strong primary X-rays generated from an X-ray tube to obtain characteristic X-rays specific to the element. The X-rays are introduced into a spectrometer and the wavelength is analyzed to determine the Ca intensity (Ca content). The metal soap content in the polyethylene resin composition is calculated from this content.

[0392] ((3) Aspect ratio of strand accumulation during twin-screw extrusion)

[0393] <Twin-screw extrusion conditions>

[0394] The slurry is obtained by mixing a polyethylene resin composition (ultra-high molecular weight polyethylene powder and metal soap) and liquid paraffin within the range of the following (Formula I) and (Formula II).

[0395] That is, the polymer concentration is adjusted to be greater than or equal to the value of Formula I and less than or equal to the value of Formula II.

[0396] Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight (Mv)

[0397] Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight (Mv)

[0398] The amount of the metal soap contained in the slurry was 5% by mass relative to the mass of the ultra-high molecular weight polyethylene powder.

[0399] Next, the slurry was kneaded and extruded using a Labo Plastomill (main body model: 4C150) manufactured by Toyo Seiki Co., Ltd. with a counter-rotating twin-screw extruder (main body model: 2D25S) to obtain a strand deposit.

[0400] It should be noted that a counter-rotating twin-screw extruder is used as the twin-screw extruder, the extrusion temperature is 160°C, the screw speed is 150rpm, the aperture of the discharge port is 1.0mm, the height from the discharge port to the ground is 1.0m to 1.1m, the discharge volume is 0.5kg / hour to 5.0kg / hour, the extrusion time is 1 hour, the atmosphere temperature and humidity are 15°C to 30°C, 20%RH to 70%RH, and the table top is made of aluminum.

[0401] As described above, the aspect ratio of the obtained strand deposit is as follows: Figure 1 As shown, the maximum height of the accumulation in the direction perpendicular to the ground is set as the vertical (H), and the maximum spreading width in the direction horizontal to the ground is set as the horizontal (W), and the vertical height is divided by the horizontal spreading width to calculate (vertical height / horizontal spreading width = H / W). For the vertical (H), it is set to the maximum height from the table to the top of the wire accumulation, and for the horizontal (W), the equivalent circle diameter of the bottom cross section is calculated from the observation image obtained by photographing the bottom cross section of the wire accumulation using image analysis software (manufactured by Asahi Kasei Corporation, A-image version 2.50) and is used as W.

[0402] ((4) Method for extracting metal soap from polyethylene resin composition)

[0403] The metal soap was extracted from the polyethylene resin composition under the conditions shown below.

[0404] The polyethylene resin composition was placed in a mixed solvent of chloroform / propylene glycol (9 / 1: unit is mass %), stirred at room temperature for 30 minutes to 1 hour, and then suction filtered.

[0405] The obtained solvent was subjected to boiling point control in an evaporator under reduced pressure and heating to remove chloroform, and then suction filtration was performed while washing with ethanol to obtain a metal soap.

[0406] The metal soap extracted in (4) is used for the measurement of ((7) the content of the fatty acid having 16 or 18 carbon atoms in the metal soap) described later.

[0407] ((5) Average number of carbon atoms per alkyl chain of metal soap and ratio of C18 / C16)

[0408] The metal soap extracted from the polyethylene resin composition by the method described in (4) above was analyzed using gas chromatography (GC), thereby calculating the mass ratio of fatty acids with 18 carbon atoms per alkyl chain (C18) to fatty acids with 16 carbon atoms per alkyl chain (C16): C18 / C16.

[0409] Weigh 100 mg of metal soap accurately and take it to a small conical flask equipped with a reflux condenser. Add 5.0 mL of boron trifluoride methanol reagent and shake well, and heat for about 10 minutes until dissolved. Add 4.0 mL of heptane from the condenser and heat for about 10 minutes. After cooling, add 20 mL of saturated sodium chloride solution and shake well, and let it stand to separate the liquid into two layers. The separated heptane layer is passed through about 0.1 g of anhydrous sodium sulfate that has been previously washed with heptane and taken to another flask. Take 1.0 mL of this liquid to a 10 mL volumetric flask, add heptane to make it accurately 10 mL and shake well to prepare a sample solution.

[0410] 1 μL of the sample solution was tested by gas chromatography under the following conditions.

[0411] The peak area A of methyl stearate and the peak area B of all fatty acid esters obtained in the sample solution (total detected peak areas) were measured, and the ratio (mass %) of stearic acid in the fatty acid component of the metal soap was calculated according to the following formula.

[0412] Stearic acid ratio (mass %) = A / B × 100

[0413] Similarly, the ratio (mass %) of palmitic acid contained in the metal soap was calculated.

[0414] The peak area of ​​methyl stearate is 40% or more of the total peak area of ​​all fatty acid esters obtained from the chromatogram, and the total peak area of ​​methyl stearate and methyl palmitate is 90% or more of the total peak area of ​​all fatty acid esters obtained from the chromatogram.

[0415] It should be noted that the measurement solution contains some other higher fatty acids in addition to stearic acid and palmitic acid, so while testing the content of stearic acid and palmitic acid by gas chromatography, the amount of other higher fatty acids was set to 10% by mass or less.

[0416] <Operation conditions>

[0417] Detector: Hydrogen flame ionization detector maintained at approximately 260°C

[0418] Sample introduction: Splitless injection section maintained at approximately 220°C

[0419] Column: A column obtained by coating the inner surface of a quartz column having an inner diameter of about 0.32 mm and a length of about 30 m with polyethylene glycol 15000-diepoxide for gas chromatography at a thickness of 0.5 μm.

[0420] Column temperature: maintained at 70°C for about 2 minutes after the sample was injected, then increased to 240°C at a rate of 5°C per minute, and then maintained at this temperature for 5 minutes.

[0421] Carrier gas: Helium

[0422] Flow rate: Constant flow rate of about 50 cm per second

[0423] Selection of columns: The following columns were used: About 50 mg of stearic acid for gas chromatography and about 50 mg of palmitic acid for gas chromatography, which had been dried for 4 hours using a desiccant (silica gel), were accurately weighed and placed in a small conical flask equipped with a reflux condenser. 5.0 ml of boron trifluoride·methanol test solution was added and shaken well, and the following operations were performed in the same manner as the sample solution to prepare a device adjustment solution. When 1 μL of the liquid was operated under the above operating conditions, the relative retention time ratio of methyl palmitate to methyl stearate was about 0.86, and the resolution was 5.0 or more.

[0424] Reproducibility of the test: When the device adjustment solution was repeatedly tested 6 times under the above conditions, the relative standard deviation of the peak areas of methyl palmitate and methyl stearate was less than 6.0%. In addition, the relative standard deviation of the area ratio of the peak of methyl palmitate to the peak of methyl stearate obtained by the repeated test was less than 1.0%.

[0425] ((6) Ca ion concentration of metal soap (mg / L))

[0426] The Ca ion concentration of the metal soap in the polyethylene resin composition was calculated by chelate titration.

[0427] 0.5 g of the metal soap extracted from the polyethylene resin composition by the method described in (4) above was accurately weighed into a small crucible and burned using an electric heater.

[0428] After smoke appears, light it on fire and let it burn completely.

[0429] The precipitate was placed in an electric furnace (800° C.) for 30 minutes to be incinerated, and then taken out of the furnace to be cooled naturally.

[0430] 1.5 mL of hydrochloric acid was added to the incinerated product, and 1.0 mL of ion exchange water was added, followed by heating and dissolution using an electric heater for 5 minutes.

[0431] While washing the contents of the small crucible with a small amount of ion-exchanged water, they were poured into a conical flask (300 mL), and about 95 mL of ion-exchanged water was added to adjust the volume to 100 mL.

[0432] 10.0 mL of buffer (ammonium chloride·ammonia solution) was added using a graduated pipette (25 mL).

[0433] Add 4 to 5 drops of EBT (Eriochrome Black T) indicator, titrate with a burette (50 mL) using a 0.05 mol / L EDTA standard solution, and read the titration amount when the color changes from red to blue while shaking the conical flask.

[0434] ((7) Content of fatty acid having 16 or 18 carbon atoms in metal soap (mass %))

[0435] The content (mass %) of the fatty acid having 16 or 18 carbon atoms contained in the metal soap in the polyethylene resin composition was calculated by the following method.

[0436] First, the free fatty acid contained in 1.0 g of the metal soap extracted from the polyethylene resin composition by the method described in (4) above is calculated according to the mass percentage of stearic acid, thereby obtaining the mass of the fatty acid having 16 or 18 carbon atoms contained in the metal soap in the polyethylene resin composition.

[0437] 2.0 g of the metal soap extracted from the polyethylene resin composition by the method described in (4) above was accurately weighed into a conical flask (300 mL). 95 mL of acetone for free fatty acid (FFA) measurement measured by a measuring cylinder was added, and the mixture was dispersed by shaking several times by hand and left at room temperature for 60 minutes.

[0438] The liquid was filtered using filter paper (ADVANTEC No. 2).

[0439] Then, the sample remaining at the bottom of the Erlenmeyer flask was washed with 5.0 mL of FFA measurement acetone, and the washed sample was filtered.

[0440] Weigh 100 mL of acetone for FFA measurement in a conical flask, add 3 to 4 drops of phenolphthalein indicator, and titrate with a 0.1 mol / L potassium hydroxide ethanol solution using a burette (5 mL). Shake the conical flask and a light red color will appear. Read the titration amount B mL when it lasts for 30 seconds.

[0441] Next, add 3 to 4 drops of phenolphthalein indicator to the filtered filtrate. Use a burette (5 mL) and titrate with 0.1 mol / L potassium hydroxide ethanol solution. While shaking the conical flask, a light red color is displayed. Read the titration amount AmL at the time of 30 seconds. Calculate the free fatty acid (mass %) by the following formula.

[0442] F×2.743×(A-BmL) / 2g (mass of the metal soap as a sample)

[0443] (F: factor)

[0444] ((8) Crystallinity of polyethylene resin composition (%))

[0445] The crystallinity of the polyethylene resin composition was measured by wide angle X-ray scattering (WAXS) under the following conditions.

[0446] Ultima-IV manufactured by Rigaku Corporation was used for the measurement.

[0447] Cu-Kα rays were incident on the polyethylene resin composition as a sample, and diffracted light was detected by D / tex Uitra.

[0448] The measurement conditions were set to a distance of 285 mm between the sample and the detector, an excitation voltage of 40 kV, and a current of 40 mA.

[0449] A focusing optical system was used as the optical system, and the slit conditions were DS = 1 / 2°, SS = release, and longitudinal slit = 10 mm.

[0450] ((9) Ti and Al contents in polyethylene resin composition (ppm))

[0451] The polyethylene resin composition of this embodiment was pressurized and decomposed using a microwave decomposition device (model ETHOS TC, manufactured by Milestone General), and the element concentrations of titanium (Ti) and aluminum (Al) as metal-containing materials in the polyethylene resin composition were measured using an ICP-MS (inductively coupled plasma mass spectrometer, model X series X7, manufactured by Thermo Fisher Scientific) by the internal standard method.

[0452] ((10) Method for producing microporous membrane for secondary battery separator)

[0453] A microporous film for a secondary battery separator was produced using the polyethylene resin composition.

[0454] The total amount of the polyethylene resin composition and the liquid paraffin is set to 100 parts by mass, and 5 to 50 parts by mass of ultra-high molecular weight polyethylene powder, 50 to 95 parts by mass of liquid paraffin (manufactured by Matsumura Petroleum Research Institute Co., Ltd., liquid paraffin (product name: SMOIL P-350P)) and 1 part by mass of an antioxidant (manufactured by Ohko Chemical Japan Co., Ltd., tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane (product name: ANOX20)) are blended to prepare a slurry-like liquid.

[0455] It should be noted that the detailed polymer concentration is as described in the above (3).

[0456] The obtained slurry-like liquid was replaced with nitrogen and then fed into a Labo Plastomill (main model: 4C150) manufactured by Toyo Seiki Co., Ltd. through a feeder under a nitrogen atmosphere. The mixture was kneaded at 200°C and then extruded from a T-die provided at the front end of the extruder. The mixture was then immediately cooled and solidified using a casting roll cooled to 25°C to form a gel-like sheet.

[0457] The gel-like sheet was stretched to 7×7 times using a synchronous twin-screw stretcher at 120°C, and then the stretched film was immersed in dichloromethane or hexane to extract and remove liquid paraffin, and then vacuum dried for more than 24 hours. Then, it was heat-set at 125°C for 3 minutes to obtain a microporous membrane for a secondary battery separator.

[0458] ((11) Scaling inhibition effect)

[0459] According to the twin-screw extrusion method described in (3) above, the extrusion operation is carried out for 1 hour while keeping the discharge volume and the atmospheric temperature and humidity consistent. Then, the mass of the scale attached to the front end of the hole is measured to determine whether there is a scale inhibition effect.

[0460] (Evaluation Criteria)

[0461] A (good) ... the amount of fouling is less than 15 mg / hour

[0462] B (normal) ... the amount of fouling is greater than or equal to 15 mg / hour and less than 20 mg / hour

[0463] C (poor) ... the amount of fouling is more than 20 mg / hour

[0464] ((12) Amount of metal soap in microporous membrane)

[0465] The microporous membrane for secondary battery separator manufactured by the method described in (10) above was pressurized and decomposed using a microwave decomposition device (model ETHOS TC, manufactured by Milestone General), and the element concentration of metal-containing calcium (Ca) in the microporous membrane was measured by the internal standard method using ICP-MS (inductively coupled plasma mass spectrometer, model X series X7, manufactured by Thermo Fisher Scientific) and calculated as the amount of metal soap.

[0466] (Evaluation Criteria)

[0467] A (good) ... less than 100 ppm

[0468] B (normal) ... greater than or equal to 100ppm and less than 200ppm

[0469] C (difference) ... 200ppm or more

[0470] ((13) Withstand voltage of microporous membrane)

[0471] The microporous membrane produced by the method described in (10) above was sandwiched between aluminum electrodes having a diameter of 4 cm, a load of 15 g was applied, and the electrodes were connected to a withstand voltage tester (TOS9201) manufactured by Kikusui Electronics Co., Ltd. for measurement.

[0472] The measurement conditions were set as follows: an AC voltage (60 Hz) was applied at a rate of 1.0 kV / sec, and the voltage value at the time of short circuit was defined as the withstand voltage (kV) of the film.

[0473] (Evaluation Criteria)

[0474] A (good) ... 1.0kV or more

[0475] B (normal) …… 0.5kV or more and less than 1.0kV

[0476] C(difference)……less than 0.5kV

[0477] [Catalyst synthesis method]

[0478] [Preparation of solid catalyst component [A]]

[0479] ((1) Synthesis of raw material (a-1))

[0480] 2,000 mL of 1 mol / L Mg6(C4H9) was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 12A hexane solution of Al(C2H5)3 (equivalent to 2000 mmol in total of magnesium and aluminum) was stirred at 80°C while 240 mL of a hexane solution of 8.33 mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pressure-fed, and stirring was continued at 80°C for 2 hours.

[0481] After the reaction was completed, the reaction solution cooled to room temperature was used as the raw material (a-1).

[0482] The total concentration of magnesium and aluminum in the raw material (a-1) was 0.786 mol / L.

[0483] ((2) Preparation of solid catalyst component [A])

[0484] 1,600 mL of hexane was added to an 8 L stainless steel autoclave purged with nitrogen, and 800 mL of a 1 mol / L hexane solution of titanium tetrachloride and 800 mL of the raw material (a-1) were added simultaneously over 5 hours while stirring at 10°C.

[0485] The reaction was continued for 1 hour at 10° C. After the reaction was completed, the supernatant of the obtained reaction solution was removed and washed with hexane four times to remove unreacted raw material components, thereby preparing a solid catalyst component [A].

[0486] [Preparation of solid catalyst component [B]]

[0487] ((1) Synthesis of raw material (b-1))

[0488] 2,000 mL of 1 mol / L Mg6(C4H9) was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 12 To a hexane solution of Al(C2H5)3 (equivalent to 2000 mmol in total of magnesium and aluminum), 146 mL of a 5.47 mol / L n-butanol hexane solution was added dropwise over 3 hours while stirring at 50°C. After the addition was completed, the pipeline was washed with 300 mL of hexane.

[0489] Then, stirring was continued for 2 hours at 50° C. After the reaction was completed, the reaction solution was cooled to room temperature and used as a raw material (b-1).

[0490] The raw material (b-1) had a magnesium concentration of 0.704 mol / L.

[0491] ((2) Synthesis of raw material (b-2))

[0492] 2,000 mL of 1 mol / L Mg6(C4H9) was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 12A hexane solution of Al(C2H5)3 (equivalent to 2000 mmol in terms of the total amount of magnesium and aluminum) was stirred at 80°C while pressure feeding 240 mL of a hexane solution of 8.33 mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.), and stirring was continued at 80°C for 2 hours. After the reaction was completed, the reaction solution was cooled to room temperature and used as raw material (b-2).

[0493] The total concentration of magnesium and aluminum in the raw material (b-2) was 0.786 mol / L.

[0494] ((3) (B-1) Synthesis of carrier)

[0495] 1,000 mL of a 1 mol / L hexane solution of hydroxytrichlorosilane was placed in an 8 L stainless steel autoclave that had been fully purged with nitrogen, and 1,340 mL of a hexane solution of an organic magnesium compound (equivalent to 943 mmol of magnesium) as a raw material (b-1) was added dropwise at 65° C. over 3 hours, and the reaction was continued while stirring at 65° C. for another hour. After the reaction was completed, the supernatant of the obtained reaction solution was removed, and the reaction mixture was washed four times with 1,800 mL of hexane to obtain a carrier (B-1).

[0496] The carrier (B-1) was analyzed and found to contain 7.5 mmol of magnesium per 1 g of the solid.

[0497] ((4) Preparation of solid catalyst component [B])

[0498] While stirring 1,970 mL of a hexane slurry containing 110 g of the support (B-1) at 10°C, 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of the raw material (b-2) were added simultaneously over 3 hours.

[0499] After the addition, the reaction was continued for 1 hour at 10° C. After the reaction was completed, the supernatant of the obtained reaction solution was removed and washed four times with hexane to remove unreacted raw material components, thereby preparing a solid catalyst component [B].

[0500] [Manufacturing of polyethylene resin composition]

[0501] (Example 1)

[0502] Hexane, ethylene, hydrogen and a catalyst were continuously supplied to a 300 L container-type polymerization reactor (1) equipped with a stirring device. The polymerization pressure was 0.5 MPa. The polymerization temperature was maintained at 83° C. by jacket cooling.

[0503] Hexane was supplied from the bottom of the polymerization reactor (1) at 40 L / hour. The solid catalyst component [A] was used as a catalyst, and a mixture of triisobutylaluminum and diisobutylaluminum hydride (a mixture of 9:1 in mass ratio) was used as a co-catalyst.

[0504] The solid catalyst component [A] was added at a rate of 0.2 g / hour from the middle of the liquid surface and the bottom of the polymerization reactor (1), and the co-catalyst was added at a rate of 10 mmol / hour from the middle of the liquid surface and the bottom of the polymerization reactor (1).

[0505] The production rate of polyethylene was 14 kg / hour.

[0506] Hydrogen was continuously supplied by a pump so that the hydrogen concentration relative to ethylene in the gas phase was 11.0 mol%. Hydrogen was supplied to the gas phase, and ethylene was supplied from the bottom of the polymerization reactor (1).

[0507] The catalyst activity was 50,000 g-PE / g-solid catalyst component [A].

[0508] Next, the polymerization slurry was continuously extracted into a flash tank at a pressure of 0.05 MPa and a temperature of 83° C. so as to keep the liquid level of the polymerization reactor constant, and unreacted ethylene and hydrogen were separated.

[0509] Next, the polymerization slurry was continuously fed to a centrifuge to keep the liquid level in the polymerization reactor constant, and the polyethylene powder was separated from the solvent and the like other than the polyethylene powder. The content of the solvent and the like relative to the polyethylene powder was 45% by mass.

[0510] The separated polyethylene powder was dried at 108° C. while blowing nitrogen. In this drying step, steam was sprayed onto the polymerized powder to deactivate the catalyst and the co-catalyst. The total drying time was 2 hours.

[0511] 0.150 mass % of calcium stearate (C18 / C16 ratio: 69.3) was added to the obtained polyethylene powder, and the mixture was uniformly mixed using a Henschel mixer.

[0512] The polyethylene resin composition (A-1) was obtained by removing the powder that did not pass through the sieve from the obtained polyethylene powder using a sieve having a mesh size of 425 μm.

[0513] The viscosity average molecular weight (Mv) is 30×10 4 .

[0514] In addition, the properties of the obtained polyethylene resin composition were measured by the above-mentioned methods.

[0515] The measurement results are shown in Table 2 below.

[0516] The above calcium stearate (C18 / C16 ratio: 69.3) was obtained by the method shown below.

[0517] Molten stearic acid (C18 is 97% by mass, C16 is 1.4% by mass, and the C18 / C16 mass ratio is 69.3) at a temperature of 80°C to 90°C is quantitatively supplied at a rate of 325 kg per hour, calcium hydroxide is supplied at a rate of 44 kg per hour, and acetic acid is supplied at a rate of 0.2% relative to the total amount of the mixture to a continuous mixing pin mill heated to about 120°C by a steam jacket and having a rotor speed of about 1000 rpm (peripheral speed of about 12 m / sec). The premixture continuously discharged after a residence time of 5 to 10 seconds is quenched and solidified at a rate of 4.0°C / min, and then pulverized by an atomizing mill to obtain a powdery precision mixture.

[0518] Next, 100 g of the obtained precise mixture was taken out and put into a 1 L juicer mixer with 5 g of water and stirred. 2 g of water was added 10 minutes after the start of stirring, and stirring was continued, resulting in a white powder. Methanol was sprayed on the obtained white powder and stirred, and then dried at 100° C. to obtain calcium stearate.

[0519] The aspect ratio of the strand deposit of the polyethylene resin composition of Example 1 during twin-screw extrusion was calculated by the method described in ((3) Aspect ratio of strand deposit during twin-screw extrusion).

[0520] The test was performed under the following conditions: the height from the discharge port to the ground was 1.05 m, the discharge rate was 2.5 (±0.5) kg / hour, and the atmosphere temperature and humidity were 25° C. / 60% RH.

[0521] Table 2 shows the measurement results.

[0522] The method for extracting the metal soap from the polyethylene resin composition described in Example 1 was carried out according to the method described in the above section ((4) Method for extracting the metal soap from the polyethylene resin composition, content of the metal soap).

[0523] The polyethylene resin composition described in Example 1 was stirred for 1 hour in a mixed solvent of chloroform / propylene glycol (9 / 1), and suction filtered. Methanol was then added to the obtained solvent to reprecipitate the mixture, and suction filtered again to obtain a metal soap.

[0524] The C18 / C16 ratio of the metal soap obtained in the above manner was calculated according to the method described in ((5) Average number of carbon atoms per alkyl chain of the metal soap and C18 / C16 ratio). The measurement results are shown in Table 2.

[0525] The Ca ion concentration of the metal soap obtained as described above was calculated according to the method described in ((6) Ca ion concentration of metal soap).

[0526] The fatty acid content of the metal soap obtained as described above was calculated according to the method described in the above section ((7) Content of fatty acid having 16 or 18 carbon atoms in metal soap).

[0527] The fouling evaluation of the polyethylene resin composition was performed by the method described in ((11) Fouling inhibition effect) above, and the amount of fouling attached to the tip of the hole was weighed and calculated.

[0528] The amount of metal soap in the film produced using the polyethylene resin composition was calculated by the method described in ((12) Amount of metal soap in microporous film).

[0529] The withstand voltage of the film produced using the polyethylene resin composition was calculated by the method described in ((13) Withstand voltage of microporous film).

[0530] (Example 2)

[0531] A polyethylene resin composition was obtained in the same manner as described above (Example 1), except that the polymerization pressure was set to 0.35 MPa, the polymerization temperature was set to 78°C, the hydrogen concentration relative to ethylene in the gas phase was set to 4.5 mol% and calcium stearate (C18 / C16 ratio of 2.1) was used.

[0532] It should be noted that, for calcium stearate (C18 / C16 ratio of 2.1), the same method as in Example 1 was used except that stearic acid (C18 is 67% by mass, C16 is 32% by mass, and C18 / C16 mass ratio is 2.1) was used as the raw material fatty acid to obtain calcium stearate of Example 2.

[0533] The aspect ratio of the strand deposit during twin-screw extrusion of the polyethylene resin composition of Example 2, the method for extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in [Example 1]. The measurement results are shown in Table 2.

[0534] (Example 3)

[0535] A polyethylene resin composition was obtained in the same manner as in Example 1 except that the polymerization pressure was 0.35 MPa, the polymerization temperature was 75°C, and the hydrogen concentration relative to ethylene in the gas phase was 3.8 mol %.

[0536] The aspect ratio of the strand deposit during twin-screw extrusion of the polyethylene resin composition of Example 3, the method for extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in [Example 1]. The measurement results are shown in Table 2.

[0537] (Example 4)

[0538] A polyethylene resin composition was obtained in the same manner as in Example 2 except that the polymerization pressure was 0.35 MPa, the polymerization temperature was 72° C., and the hydrogen concentration relative to ethylene in the gas phase was 0.1 mol %.

[0539] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 4, the method of extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in [Example 1]. The measurement results are shown in Table 2.

[0540] (Example 5)

[0541] A polyethylene resin composition was obtained in the same manner as in Example 1 except that the polymerization pressure was set to 0.35 MPa, the polymerization temperature was set to 50°C, the hydrogen concentration relative to ethylene in the gas phase was set to 0 mol% and calcium stearate (C18 / C16 ratio: 1.4) was used.

[0542] It should be noted that, for calcium stearate (C18 / C16 ratio of 1.4), the same method as above (Example 1) was carried out except that stearic acid (C18 is 55% by mass, C16 is 38% by mass, and C18 / C16 mass ratio is 1.4) was used as the raw material fatty acid and the speed of cooling the premix was set to 0.2°C / min, thereby obtaining calcium stearate of Example 5.

[0543] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 5, the method of extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in Example 1. The measurement results are shown in Table 2.

[0544] (Example 6)

[0545] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium behenate was used as the metal soap.

[0546] In addition, calcium behenate was obtained as a metal soap in the same manner as in the above (Example 1) except that behenic acid was used as the raw material fatty acid.

[0547] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 6, the method of extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in the above (Example 1). The measurement results are shown in Table 2.

[0548] (Example 7)

[0549] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium montanate was used as the metal soap.

[0550] In addition, calcium montanate was obtained by carrying out the same operation as in the above (Example 1) except that montanic acid was used as the raw material fatty acid.

[0551] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 7, the method of extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in the above (Example 1). The measurement results are shown in Table 2.

[0552] (Example 8)

[0553] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium stearate (C18 / C16 ratio: 0.04) was used as the metal soap.

[0554] It should be noted that calcium stearate (C18 / C16 ratio is 0.04) was prepared in the same manner as in Example 1, except that stearic acid (C18 is 4% by mass, C16 is 96% by mass, and C18 / C16 mass ratio is 0.04) was used as a raw material fatty acid and dried without blowing methanol.

[0555] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 8, the method of extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in the above-mentioned [Example 1]. The measurement results are shown in Table 2.

[0556] (Example 9)

[0557] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium stearate (C18 / C16 ratio: 0.25) was used as the metal soap.

[0558] It should be noted that, for calcium stearate (C18 / C16 ratio of 0.25), stearic acid (C18 is 20% by mass, C16 is 80% by mass, and C18 / C16 mass ratio is 0.25) was used as the raw material fatty acid, and the speed of cooling the premix was set to 0.2°C / min. Except for this, the same operation as above (Example 1) was performed to obtain calcium stearate.

[0559] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 9, the method of extracting the metal soap, the C18 / C16 ratio of the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in [Example 1]. The measurement results are shown in Table 2.

[0560] (Example 10)

[0561] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that zinc stearate (C18 / C16 ratio: 2.1) was used as the metal soap.

[0562] In addition, zinc stearate (C18 / C16 ratio: 2.1) was obtained by the method shown below.

[0563] 325 kg per hour of molten stearic acid (C18 is 67% by mass, C16 is 32% by mass, and the C18 / C16 mass ratio is 2.1) at a temperature of 80°C to 90°C, 44 kg per hour of zinc oxide, and 0.4% by mass of acetic acid relative to the total amount of the mixture are quantitatively supplied to a continuous mixing pin mill heated to about 120°C by a steam jacket and having a rotor speed of about 1000 rpm (peripheral speed of about 12 m / sec). The premixture continuously discharged after a residence time of 5 to 10 seconds is quenched and solidified at a rate of 4.0°C / min, and then pulverized by an atomizing mill to obtain a powdery precision mixture.

[0564] Next, 100 g of the obtained mixture was taken out and put into a juicer mixer with a capacity of 1 L together with 5 g of water, and stirred. 2 g of water was added 10 minutes after the start of stirring, and stirring was further continued to obtain a white powder.

[0565] Methanol was blown into the obtained white powder, the mixture was stirred, and then dried at 80° C., thereby obtaining zinc stearate.

[0566] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Example 10, the method of extracting the metal soap, the C18 / C16 ratio of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in the above (Example 1). The measurement results are shown in Table 2.

[0567] (Comparative Example 1)

[0568] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium palmitate (C16 / C14 mass ratio: 1.2) was used as the metal soap.

[0569] It should be noted that for calcium palmitate (C16 / C14 mass ratio of 1.2), palmitic acid (C16 is 55 mass%, C14 is 45 mass%, C16 / C14 mass ratio is 1.2) is used as the raw fatty acid, drying is carried out without blowing methanol, and the cooling rate of the premix is ​​set to 0.2°C / min. Except for this, the same operation as above (Example 1) is performed to obtain calcium palmitate.

[0570] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Comparative Example 1, the method of extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in Example 1. The measurement results are shown in Table 3.

[0571] (Comparative Example 2)

[0572] A polyethylene resin composition was obtained in the same manner as in Example 1 except that the polymerization pressure was 0.35 MPa, the polymerization temperature was 48° C., the hydrogen concentration relative to ethylene in the gas phase was 0 mol %, and calcium laurate was used as the metal soap.

[0573] Calcium laurate was obtained in the same manner as in Example 1, except that the fatty acid as a raw material was changed to lauric acid, the drying was performed without blowing methanol, and the cooling rate of the premix was set to 0.2° C. / min.

[0574] The aspect ratio of the strand deposit during twin-screw extrusion of the polyethylene resin composition described in Comparative Example 2, the method for extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in Example 1. The measurement results are shown in Table 3.

[0575] (Comparative Example 3)

[0576] A polyethylene resin composition was obtained in the same manner as described above (Example 1), except that the polymerization pressure was set to 0.5 MPa, the polymerization temperature was set to 83°C, the hydrogen concentration relative to ethylene in the gas phase was set to 20.0 mol% and calcium palmitate (C16 / C14 mass ratio of 1.2) was used as the metal soap.

[0577] It should be noted that, for calcium palmitate (C16 / C14 ratio of 1.2) as a metal soap, palmitic acid (C16 is 55% by mass, C14 is 45% by mass, and C16 / C14 mass ratio is 1.2) is used as a raw fatty acid, and drying is performed without blowing methanol, and the cooling rate of the premix is ​​set to 0.2°C / min. Except for this, the same operation as above (Example 1) is performed to obtain calcium palmitate.

[0578] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Comparative Example 3, the method of extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in Example 1. The measurement results are shown in Table 3.

[0579] (Comparative Example 4)

[0580] A polyethylene resin composition was obtained in the same manner as in the above (Example 1) except that calcium palmitate (C16 / C14 mass ratio: 1.2) was used as the metal soap.

[0581] It should be noted that for calcium palmitate (C16 / C14 mass ratio of 1.2), palmitic acid (C16 is 55 mass%, C14 is 45 mass%, C16 / C14 mass ratio is 1.2) is used as the raw fatty acid, and the speed of cooling the premix is ​​set to 0.2°C / min. Except for this, the same method as above (Example 1) is carried out to obtain calcium palmitate.

[0582] The aspect ratio of the strand deposit during the twin-screw extrusion of the polyethylene resin composition described in Comparative Example 4, the method of extracting the metal soap, the Ca ion concentration of the metal soap, the fatty acid content of the metal soap, the fouling evaluation, the amount of metal soap in the film, and the withstand voltage of the film were calculated in the same manner as in Example 1. The measurement results are shown in Table 3.

[0583]

[0584]

[0585] [Table 4]

[0586] Fatty acid raw materials ① ② ③ ④ ⑤ ⑥ C18 97 67 55 4 20 – C16 1.4 32 38 96 80 55 C14 – – – – – 45 C18 / C16 69.3 2.1 1.4 0.04 0.25 – C16 / C14 – – – – – 1.2

[0587] Industrial Applicability

[0588] The polyethylene resin composition of the present invention has industrial applicability as a raw material for various molded products, microporous films, separators, and high-strength fibers.

Claims

1. A polyethylene resin composition, comprising an ultra-high molecular weight polyethylene powder and a metal soap, wherein: The viscosity average molecular weight Mv of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and When the polyethylene resin composition is subjected to twin-screw extrusion under the following twin-screw extrusion conditions, the aspect ratio of the strand deposit is vertical / horizontal = 0.05 or more and 7.0 or less, Twin screw extrusion conditions Polymer concentration: According to the viscosity average molecular weight Mv of the polyethylene resin composition, The polymer concentration is adjusted to be above the value of formula I and below the value of formula II, Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight Mv Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight Mv Polyethylene resin composition: 5% to 50% by mass Liquid paraffin: 50% to 95% by mass Extruder: Counter-rotating twin-screw extruder Extrusion temperature: 160℃ Screw speed: 150rpm The diameter of the discharge port: 1.0mm Addition amount of metal soap: Add 5% of metal soap relative to the mass of ultra-high molecular weight polyethylene powder Height from outlet to ground: 1.0m or more and 1.1m or less Discharge: 0.5kg / hour or more and 5.0kg / hour or less Squeeze time: 1 hour Atmospheric temperature and humidity: 15°C or higher and 30°C or lower, 20%RH or higher and 70%RH or lower Table material: aluminum plate.

2. The polyethylene resin composition according to claim 1, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 900×10 4 the following.

3. The polyethylene resin composition according to claim 1 or 2, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 800×10 4 the following.

4. The polyethylene resin composition according to claim 1 or 2, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 500×10 4 the following.

5. The polyethylene resin composition according to claim 1, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and less than 300×10 4 .

6. The polyethylene resin composition according to claim 1 or 5, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 200×10 4 the following.

7. The polyethylene resin composition according to claim 1, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 300×10 4 Above and 1000×10 4 the following.

8. The polyethylene resin composition according to claim 1 or 7, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 300×10 4 Above and 800×10 4 the following.

9. The polyethylene resin composition according to claim 1 or 2, wherein: The ultra-high molecular weight polyethylene powder is a powder containing an ethylene homopolymer.

10. The polyethylene resin composition according to claim 1 or 2, wherein The ultra-high molecular weight polyethylene powder is a powder containing a copolymer of ethylene and an olefin copolymerizable with ethylene.

11. The polyethylene resin composition according to claim 10, wherein The olefin copolymerizable with ethylene is selected from α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, 1 and at least one comonomer selected from the group consisting of a compound represented by and a linear, branched or cyclic diene having 3 to 15 carbon atoms, wherein R 1 It is an aryl group having 6 to 12 carbon atoms.

12. The polyethylene resin composition according to claim 11, wherein The α-olefin is at least one selected from the group consisting of propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.

13. The polyethylene resin composition according to claim 10, wherein The content of the comonomer unit is 0.01 mol% or more and 5 mol% or less.

14. The polyethylene resin composition according to claim 10, wherein The content of the comonomer unit is 0.01 mol% or more and 2 mol% or less.

15. The polyethylene resin composition according to claim 10, wherein The content of the comonomer unit is 0.01 mol% or more and 1 mol% or less.

16. The polyethylene resin composition according to claim 1 or 2, wherein: The strand deposit has an aspect ratio of length / width=0.05 or more and 5.0 or less.

17. The polyethylene resin composition according to claim 1 or 2, wherein: The strand deposit has an aspect ratio of length / width=0.05 or more and 4.0 or less.

18. The polyethylene resin composition according to claim 1 or 2, wherein: The strand deposit has an aspect ratio of length / width=0.07 or more and 3.0 or less.

19. The polyethylene resin composition according to claim 1 or 2, wherein: The strand deposit has an aspect ratio of length / width=0.1 or more and 2.0 or less.

20. The polyethylene resin composition according to claim 1 or 2, wherein: The discharge rate of the twin-screw extrusion conditions is 2.0 kg / hour to 3.0 kg / hour.

21. The polyethylene resin composition according to claim 1 or 2, wherein: The output under the twin-screw extrusion conditions was 2.5 kg / hour.

22. The polyethylene resin composition according to claim 1 or 2, wherein: The content of the metal soap is 0.01 mass % or more and 0.3 mass % or less.

23. The polyethylene resin composition according to claim 1 or 2, wherein: The content of the metal soap is 0.05 mass % or more and 0.25 mass % or less.

24. The polyethylene resin composition according to claim 1 or 2, wherein: The content of the metal soap is 0.1 mass % or more and 0.20 mass % or less.

25. The polyethylene resin composition according to claim 1 or 2, wherein: The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 28.0 or less.

26. The polyethylene resin composition according to claim 1 or 2, wherein: The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 22.0 or less.

27. The polyethylene resin composition according to claim 1 or 2, wherein: The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 20.0 or less.

28. The polyethylene resin composition according to claim 1 or 2, wherein: The metal soap contains a fatty acid C16 having 16 carbon atoms in each alkyl chain and a fatty acid C18 having 18 carbon atoms in each alkyl chain, and The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is 1.5 or more and 1,000 or less.

29. The polyethylene resin composition according to claim 28, wherein The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is greater than or equal to 1.5 and less than or equal to 900.

30. The polyethylene resin composition according to claim 28, wherein The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is greater than or equal to 2.0 and less than or equal to 800.

31. The polyethylene resin composition according to claim 1 or 2, wherein: The Ca ion concentration of the metal soap is 1.0 mg / L or more and 200 mg / L or less.

32. The polyethylene resin composition according to claim 1 or 2, wherein: The Ca ion concentration of the metal soap is 1.0 mg / L or more and 180 mg / L or less.

33. The polyethylene resin composition according to claim 1 or 2, wherein: The Ca ion concentration of the metal soap is 1.0 mg / L or more and 100 mg / L or less.

34. The polyethylene resin composition according to claim 1 or 2, wherein: The Ca ion concentration of the metal soap is 1.0 mg / L or more and 50 mg / L or less.

35. The polyethylene resin composition according to claim 1 or 2, wherein: The metal soap contains 0.1 mass % or more and 2.0 mass % or less of a fatty acid having 16 or 18 carbon atoms.

36. The polyethylene resin composition according to claim 1 or 2, wherein: The metal soap contains 0.1 mass % or more and 1.9 mass % or less of a fatty acid having 16 or 18 carbon atoms.

37. The polyethylene resin composition according to claim 1 or 2, wherein: The metal soap contains 0.1 mass % or more and 1.8 mass % or less of a fatty acid having 16 or 18 carbon atoms.

38. The polyethylene resin composition according to claim 1 or 2, wherein: The metal soap contains 0.1 mass % or more and 1.5 mass % or less of a fatty acid having 16 or 18 carbon atoms.

39. The polyethylene resin composition according to claim 1 or 2, wherein: The polyethylene resin composition has a crystallinity of 70% or more and 80% or less.

40. The polyethylene resin composition according to claim 1 or 2, wherein: The polyethylene resin composition has a crystallinity of 70% or more and 78% or less.

41. The polyethylene resin composition according to claim 1 or 2, wherein: The polyethylene resin composition has a crystallinity of 70% or more and 75% or less.

42. The polyethylene resin composition according to claim 1 or 2, wherein The titanium content in the polyethylene resin composition is 0.1 ppm or more and 5.0 ppm or less.

43. The polyethylene resin composition according to claim 1 or 2, wherein: The titanium content in the polyethylene resin composition is 0.5 ppm or more and 5.0 ppm or less.

44. The polyethylene resin composition according to claim 1 or 2, wherein: The titanium content in the polyethylene resin composition is 1.0 ppm or more and 4.0 ppm or less.

45. The polyethylene resin composition according to claim 1 or 2, wherein The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 5.0 ppm or less.

46. ​​The polyethylene resin composition according to claim 1 or 2, wherein: The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 4.0 ppm or less.

47. The polyethylene resin composition according to claim 1 or 2, wherein: The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 3.5 ppm or less.

48. The polyethylene resin composition according to claim 1 or 2, wherein: After the polyethylene resin composition is twin-screw extruded under the twin-screw extrusion conditions, the amount of scale attached to the front end of the hole is less than 20 mg / hour.

49. A molded body, wherein The molded article is a molded article of the polyethylene resin composition according to any one of claims 1 to 48.

50. The molded article according to claim 49, wherein The molded body is any one selected from the group consisting of a microporous film, a high-strength fiber, and a sintered body.

51. The molded article according to claim 49 or 50, wherein The molded body is a microporous membrane for a secondary battery separator.

52. The molded article according to claim 49 or 50, wherein The molded body is a microporous membrane for a lithium ion secondary battery separator.

53. The molded article according to claim 51, wherein The amount of metal soap in the microporous membrane is less than 200 ppm, and the amount of metal soap is the element concentration of calcium in the microporous membrane.

54. The molded article according to claim 51, wherein The withstand voltage of the microporous membrane is greater than or equal to 0.5 kV.

55. A polyethylene resin composition, comprising ultra-high molecular weight polyethylene powder and metal soap, wherein: The viscosity average molecular weight Mv of the polyethylene resin composition is 100,000 or more and 10,000,000 or less, and The average number of carbon atoms in each alkyl chain of the metal soap is 16.0 or more and 28.0 or less, The metal soap contains a fatty acid C16 having 16 carbon atoms in each alkyl chain and a fatty acid C18 having 18 carbon atoms in each alkyl chain, and The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is 1.5 or more and 1,000 or less.

56. The polyethylene resin composition according to claim 55, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 900×10 4 the following.

57. The polyethylene resin composition according to claim 55 or 56, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 800×10 4 the following.

58. The polyethylene resin composition according to claim 55 or 56, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 500×10 4 the following.

59. The polyethylene resin composition of claim 55, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and less than 300×10 4 .

60. The polyethylene resin composition according to claim 55 or 59, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 10×10 4 Above and 200×10 4 the following.

61. The polyethylene resin composition of claim 55, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 300×10 4 Above and 1000×10 4 the following.

62. The polyethylene resin composition according to claim 55 or 61, wherein The viscosity average molecular weight Mv of the polyethylene resin composition is 300×10 4 Above and 800×10 4 the following.

63. The polyethylene resin composition according to claim 55 or 56, wherein The ultra-high molecular weight polyethylene powder is a powder containing an ethylene homopolymer.

64. The polyethylene resin composition according to claim 55 or 56, wherein The ultra-high molecular weight polyethylene powder is a powder containing a copolymer of ethylene and an olefin copolymerizable with ethylene.

65. The polyethylene resin composition of claim 64, wherein The olefin copolymerizable with ethylene is selected from α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, 1 and at least one comonomer selected from the group consisting of a compound represented by and a linear, branched or cyclic diene having 3 to 15 carbon atoms, wherein R 1 It is an aryl group having 6 to 12 carbon atoms.

66. The polyethylene resin composition of claim 65, wherein The α-olefin is at least one selected from the group consisting of propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.

67. The polyethylene resin composition of claim 64, wherein The content of the comonomer unit is 0.01 mol% or more and 5 mol% or less.

68. The polyethylene resin composition of claim 64, wherein The content of the comonomer unit is 0.01 mol% or more and 2 mol% or less.

69. The polyethylene resin composition of claim 64, wherein The content of the comonomer unit is 0.01 mol% or more and 1 mol% or less.

70. The polyethylene resin composition according to claim 55 or 56, wherein The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 22.0 or less.

71. The polyethylene resin composition according to claim 55 or 56, wherein The average number of carbon atoms per alkyl chain of the metal soap is 16.0 or more and 20.0 or less.

72. The polyethylene resin composition according to claim 55 or 56, wherein The content of the metal soap is 0.01 mass % or more and 0.3 mass % or less.

73. The polyethylene resin composition according to claim 55 or 56, wherein The content of the metal soap is 0.05 mass % or more and 0.25 mass % or less.

74. The polyethylene resin composition according to claim 55 or 56, wherein The content of the metal soap is 0.1 mass % or more and 0.20 mass % or less.

75. The polyethylene resin composition of claim 55, wherein The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is greater than or equal to 1.5 and less than or equal to 900.

76. The polyethylene resin composition according to claim 55 or 75, wherein The mass ratio C18 / C16 of the fatty acid having 18 carbon atoms per alkyl chain to the fatty acid having 16 carbon atoms per alkyl chain is greater than or equal to 2.0 and less than or equal to 800.

77. The polyethylene resin composition according to claim 55 or 56, wherein The Ca ion concentration of the metal soap is 1.0 mg / L or more and 200 mg / L or less.

78. The polyethylene resin composition according to claim 55 or 56, wherein The Ca ion concentration of the metal soap is 1.0 mg / L or more and 180 mg / L or less.

79. The polyethylene resin composition according to claim 55 or 56, wherein The Ca ion concentration of the metal soap is 1.0 mg / L or more and 100 mg / L or less.

80. The polyethylene resin composition according to claim 55 or 56, wherein The Ca ion concentration of the metal soap is 1.0 mg / L or more and 50 mg / L or less.

81. The polyethylene resin composition according to claim 55 or 56, wherein The metal soap contains 0.1 mass % or more and 2.0 mass % or less of a fatty acid having 16 or 18 carbon atoms.

82. The polyethylene resin composition according to claim 55 or 56, wherein The metal soap contains 0.1 mass % or more and 1.9 mass % or less of a fatty acid having 16 or 18 carbon atoms.

83. The polyethylene resin composition according to claim 55 or 56, wherein The metal soap contains 0.1 mass % or more and 1.8 mass % or less of a fatty acid having 16 or 18 carbon atoms.

84. The polyethylene resin composition according to claim 55 or 56, wherein The metal soap contains 0.1 mass % or more and 1.5 mass % or less of a fatty acid having 16 or 18 carbon atoms.

85. The polyethylene resin composition according to claim 55 or 56, wherein The polyethylene resin composition has a crystallinity of 70% or more and 80% or less.

86. The polyethylene resin composition according to claim 55 or 56, wherein The polyethylene resin composition has a crystallinity of 70% or more and 78% or less.

87. The polyethylene resin composition according to claim 55 or 56, wherein The polyethylene resin composition has a crystallinity of 70% or more and 75% or less.

88. The polyethylene resin composition according to claim 55 or 56, wherein The titanium content in the polyethylene resin composition is 0.1 ppm or more and 5.0 ppm or less.

89. The polyethylene resin composition according to claim 55 or 56, wherein The titanium content in the polyethylene resin composition is 0.5 ppm or more and 5.0 ppm or less.

90. The polyethylene resin composition according to claim 55 or 56, wherein The titanium content in the polyethylene resin composition is 1.0 ppm or more and 4.0 ppm or less.

91. The polyethylene resin composition according to claim 55 or 56, wherein The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 5.0 ppm or less.

92. The polyethylene resin composition according to claim 55 or 56, wherein The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 4.0 ppm or less.

93. The polyethylene resin composition according to claim 55 or 56, wherein The aluminum content in the polyethylene resin composition is 0.1 ppm or more and 3.5 ppm or less.

94. The polyethylene resin composition according to claim 55 or 56, wherein After the polyethylene resin composition is subjected to twin-screw extrusion under the following twin-screw extrusion conditions, the amount of scale deposited on the front end of the hole is less than 20 mg / hour, Twin screw extrusion conditions Polymer concentration: According to the viscosity average molecular weight Mv of the polyethylene resin composition, The polymer concentration is adjusted to be above the value of formula I and below the value of formula II, Formula I: Y = 260.63X -0.484 , Y: polymer concentration, X: molecular weight Mv Formula II: Y = 338.69X -0.626 , Y: polymer concentration, X: molecular weight Mv Polyethylene resin composition: 5% to 50% by mass Liquid paraffin: 50% to 95% by mass Extruder: Counter-rotating twin-screw extruder Extrusion temperature: 160℃ Screw speed: 150rpm The diameter of the discharge port: 1.0mm Addition amount of metal soap: Add 5% of metal soap relative to the mass of ultra-high molecular weight polyethylene powder Height from outlet to ground: 1.0m or more and 1.1m or less Discharge: 0.5kg / hour or more and 5.0kg / hour or less Squeeze time: 1 hour Atmospheric temperature and humidity: 15°C or higher and 30°C or lower, 20%RH or higher and 70%RH or lower Table material: aluminum plate.

95. A molded body, wherein The molded article is a molded article of the polyethylene resin composition according to any one of claims 55 to 94.

96. The molded article of claim 95, wherein The molded body is any one selected from the group consisting of a microporous film, a high-strength fiber, and a sintered body.

97. The molded article according to claim 95 or 96, wherein The molded body is a microporous membrane for a secondary battery separator.

98. The molded article according to claim 95 or 96, wherein The molded body is a microporous membrane for a lithium ion secondary battery separator.

99. The molded article according to claim 97, wherein The amount of metal soap in the microporous membrane is less than 200 ppm, and the amount of metal soap is the element concentration of calcium in the microporous membrane.

100. The molded article according to claim 97, wherein The withstand voltage of the microporous membrane is greater than or equal to 0.5 kV.