Prediction method and application of compressive residual strength of CFRTP with delamination damage

By establishing the relationship between layered damage depth, ambient temperature and humidity and heat aging time and the residual strength of CFRTP compression, the problem of inaccurate prediction of the residual strength of composite materials in the prior art is solved, and accurate calculations are achieved in high temperature and humidity and heat environments and security.

CN115017699BActive Publication Date: 2024-12-03SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210624882.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-02
Publication Date
2024-12-03
Estimated Expiration
2042-06-02

AI Technical Summary

Technical Problem

The prior art lacks a calculation formula for the compression residual strength of the composite material containing layered damage. Especially in high temperature and humid and heat environments, it is impossible to accurately predict the compression residual strength of the thermoplastic resin-based composite material, resulting in safety hazards and structural use problems.

Method used

The relationship between the layered damage depth, ambient temperature and humid and heat aging time and the residual intensity of CFRTP compression was established. The compressed residual intensity of CFRTP containing stratified damage was calculated by the formula. The environmental correlation coefficient k, temperature parameters kT and humidity heat were introduced into the formula. Parameter Ks, combined with experimental values ​​and measurement data, the pending constants a and b are obtained, and the calculation results are relatively accurate.

Benefits of technology

Accurate calculations in room temperature, high temperature and humid and heat environments are achieved, which reduces the safety risks of composite materials, ensures their use safely, and provides repair methods to avoid damage and expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003676656180000011
    Figure BDA0003676656180000011
  • Figure BDA0003676656180000023
    Figure BDA0003676656180000023
  • Figure BDA0003676656180000031
    Figure BDA0003676656180000031
Patent Text Reader

Abstract

The present invention relates to a prediction method and application of the residual strength of CFRTP with delamination damage. The prediction method comprises: determining a coefficient k related to the environment (normal temperature environment, high temperature environment, humid and hot environment), a non-damaged CFRTP compressive strength σ b , the delamination damage depth d, and the total thickness h of the CFRTP with delamination damage are substituted into the formula to calculate the compressive residual strength σ of the CFRTP with delamination damage c ; Application: using the prediction method to obtain the compressive residual strength of CFRTP with delamination damage to guide the repair process of CFRTP with delamination damage. The present invention can directly calculate the influence of delamination damage depth, high temperature environment, and hot and humid environment on the compressive residual strength of CFRTP with delamination damage, judge whether there are safety hazards in the service process of CFRTP in high temperature environment and hot and humid environment, eliminate safety hazards in the use of CFRTP, and ensure its safe use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials and relates to a prediction method and application of the compression residual strength of CFRTP containing delamination damage. Background Art

[0002] Thermoplastic resins have poor fluidity. Thermoplastic resin-based composites are very prone to delamination damage during the preparation process. When they are impacted during transportation and use, delamination damage is also likely to occur inside the material. Delamination damage has a significant impact on the load-bearing capacity and service life of composite components. As the delamination damage expands and evolves, the composite material will be severely damaged until it completely fails, which is the main safety hazard of composite components. Carbon fiber reinforced thermoplastic resin-based composites (CFRTP) are currently widely used in aircraft wings, fuselage skins, cabin panels and other parts, which are often in high temperature and humid and hot environments, which will further affect the load-bearing capacity of composite structures. Therefore, establishing the relationship between delamination damage depth, ambient temperature and humid and hot aging time and CFRTP compressive residual strength is of far-reaching significance for the damage tolerance design of thermoplastic composites, the safety assurance of structural use, and repair.

[0003] At present, there is no special calculation formula for the compressive residual strength of composite materials with delamination damage. Some calculation formulas for the residual strength of composite materials with defects cannot accurately calculate the compressive residual strength of composite materials with delamination damage because they take into account various defects. The performance of thermoplastic resins and thermosetting resins in high temperature environments and hot and humid environments is quite different, and the calculation formula for the residual strength of composite materials is often not applicable to thermoplastic composites. Therefore, it is necessary to establish the compressive residual strength of CFRTP with delamination damage in high temperature environments and hot and humid environments based on the performance evolution of thermoplastic resin-based composites in high temperature environments and hot and humid environments. Summary of the invention

[0004] In order to predict the room temperature compressive residual strength of CFRTP with different depths of delamination damage (delamination at the geometric center of the material, diameter 50mm) and the compressive residual strength of CFRTP with delamination damage (delamination at the geometric center of the material, located between the 5 / 6 layers, diameter 50mm) at different temperatures and wet heat time, the present invention establishes a relationship between the delamination damage depth, ambient temperature and wet heat aging time and the compressive residual strength of CFRTP. The method is simple to calculate, does not require experiments, and the calculation results are relatively accurate.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] Prediction method for compressive residual strength of CFRTP with delamination damage, determination of environment-related coefficient k, compressive strength σ of undamaged CFRTP b, the delamination damage depth (the distance from the delamination damage to the thin sub-plate surface) d, and the total thickness h of the CFRTP with delamination damage are substituted into the formula to calculate the compressive residual strength σ of the CFRTP with delamination damage c , the formula is as follows:

[0007]

[0008] Where k is unitless; σ b The unit of is MPa; the unit of d and h is mm;

[0009] When the environment is at normal temperature, k = 1;

[0010] When the environment is high temperature, T is the ambient temperature, in °C, and its value is measured by a thermometer; T0 is the change parameter of the elastic modulus of CFRTP at high temperature, with a value of 100, in °C; E T E is the elastic modulus of the undamaged CFRTP at ambient temperature, in MPa, and is measured by the DMA (dynamic mechanical properties analysis) method; R is the elastic modulus of the undamaged CFRTP at room temperature (i.e., 25°C), in MPa, and its value is measured by the DMA (dynamic mechanical properties analysis) method;

[0011] When the environment is hot and humid, t is the value of the damp heat aging time in h, and its value is obtained by timing with a timer. For example, if the damp heat aging time is 1 h, then t is 1; e is the base of the natural logarithm function (e = 2.71828183); T is the ambient temperature in °C, and its value is obtained by measuring with a thermometer; T g T is the glass transition temperature of CFRTP, in °C, and its value is measured by DSC (differential scanning calorimetry) and DMA method; s is the parameter affecting the performance of CFRTP under the humid and hot environment, which is 10 and the unit is ℃; a and b are the unknown constants related to the humid and hot conditions, and their values ​​are obtained by dividing the σ under the specific humid and hot environment by c The experimental value of σ b The experimental values ​​of d, h, t, T, T g 、T s Substitute it into the following formula to obtain;

[0012]

[0013] The temperature of the normal temperature environment is 20-30°C, and the relative humidity is 40%-60% RH; the temperature of the high temperature environment is 60-200°C, and the relative humidity is 40%-60% RH; the temperature of the humid and hot environment is 40-100°C, and the relative humidity is 65%-100% RH.

[0014] As the preferred technical solution:

[0015] As mentioned above, the prediction method of compressive residual strength of CFRTP with delamination damage, σ b The value of is measured by ASTM D 3410-03, a standard test method for compressive properties of polymer matrix composites.

[0016] In the above-mentioned prediction method for the compressive residual strength of CFRTP with delamination damage, the value of d is obtained by measuring with a vernier caliper.

[0017] In the above-mentioned prediction method of the compressive residual strength of CFRTP with delamination damage, the value of h is obtained by measuring using non-destructive testing methods such as CT.

[0018] The formula used to predict the compressive residual strength of CFRTP with delamination damage is derived as follows:

[0019] Because stress concentration will occur near the delamination damage of CFRTP with delamination damage, the stress distribution near the damage in the softening inclusion model is regarded as the room-temperature compressive residual strength of CFRTP with delamination damage, and the calculation formula (1) for the room-temperature compressive residual strength of CFRTP with delamination damage can be obtained:

[0020]

[0021] In formula (1), σ c is the residual compressive strength of CFRTP with delamination damage, in MPa; σ b is the undamaged CFRTP compressive strength, in MPa; α k is the corrected delamination damage parameter.

[0022] When the layer shape and size are constant, the effect of the layer depth on the CFRTP compressive residual strength is roughly exponential, that is, formula (2):

[0023]

[0024] In formula (2), α is a constant related only to the delamination damage; d is the delamination damage depth (the distance from the delamination damage to the thin sub-panel surface), in mm; h is the total thickness of the composite material, in mm; the α value is determined to be 1 according to the "Guidelines for Durability / Damage Tolerance Design of Composite Aircraft Structures".

[0025] Substituting formula (2) into formula (1), we can obtain the relationship between the delamination damage depth and the residual strength of CFRTP at room temperature, namely formula (3):

[0026]

[0027] The compressive strength of the composite material is proportional to the elastic modulus of the material. As the temperature rises, the compressive residual strength of the composite material decreases slowly before the glass transition temperature and decreases rapidly after the glass transition temperature, showing a parabolic change trend. Based on this, the temperature parameter k is defined, that is, formula (4):

[0028]

[0029] In formula (4), T is the ambient temperature, in °C; T0 is the parameter affecting the elastic modulus of CFRTP, which is 100 and in °C; E T is the elastic modulus of the composite material at temperature T, in MPa; E R is the elastic modulus of the composite material at room temperature, in MPa.

[0030] Add the temperature parameter k to formula (3) T , the relationship between the compressive residual strength and temperature of CFRTP with delamination damage is obtained, that is, formula (5):

[0031]

[0032] By adding the relationship between the residual strength of the composite material and the aging time to formula (3), we can get the relationship between the compressive residual strength of the composite material with delamination damage and the wet heat aging time, that is, formula (6):

[0033]

[0034] In formula (6), t is the value of the wet heat aging time in h; a and b are unknown constants related to the wet heat conditions, and their values ​​are calculated by subtracting σ c The experimental value of σ b The experimental values ​​of d, h, t, T, T g 、T s Substitute it into the following formula to obtain;

[0035] The heat resistance of CFRTP varies greatly, and the interlayer bonding performance, interface performance and crystallinity of the composite material vary greatly at different temperatures. The change in the compressive residual strength after wet heat aging is exponentially related to the difference between the wet heat aging temperature and the glass transition temperature of the matrix resin. Based on this, the wet heat resistance parameter K is defined. s , that is, formula (7):

[0036]

[0037] In formula (7), T is the ambient temperature in °C; T g is the glass transition temperature of the material, in °C; Ts is the parameter that influences the wet-heat performance of CFRTP, with a value of 10 and a unit of ℃.

[0038] By adding the moisture and heat resistance parameters of CFRTP to formula (6), the relationship between the compressive residual strength of CFRTP with delamination damage and the moisture and heat aging time can be obtained, that is, formula (8):

[0039]

[0040] The present invention also provides a method for repairing CFRTP with delamination damage, that is, application of the above-mentioned method for predicting the compressive residual strength of CFRTP with delamination damage, comprising the following steps:

[0041] (i) using the prediction method for compressive residual strength of CFRTP with delamination damage as described in any one of the above items to obtain the compressive residual strength of CFRTP with delamination damage;

[0042] (ii) determining whether the delamination damage reaches the damage tolerance of CFRTP, if yes, proceeding to step (iii); otherwise, proceeding to step (iv);

[0043] (iii) repairing the delamination that exceeds the damage tolerance and returning to step (i);

[0044] (iv) Continue to use CFRTP.

[0045] As the preferred technical solution:

[0046] In the above-mentioned method for repairing CFRTP with delamination damage, the repair is carried out by injection resin method.

[0047] Beneficial effects:

[0048] The present invention can directly calculate the influence of the delamination damage depth, high temperature environment and humid heat environment on the compressive residual strength of CFRTP containing delamination damage, judge whether there are safety hazards in the service process of CFRTP in high temperature environment and humid heat environment, eliminate the safety hazards in the use of CFRTP, and ensure its safe use. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0050] The prediction method of residual compressive strength of CFRTP with delamination damage is used to determine the value of the coefficient k related to the environment and the compressive strength σ of undamaged CFRTP.b The value of (σ b The value of is measured by ASTM D 3410-03, the standard test method for compressive properties of polymer matrix composites), the value of the delamination damage depth (the distance from the delamination damage to the surface of the thin sub-plate) d (the value of d is measured by a vernier caliper), and the value of the total thickness h of the CFRTP with delamination damage (the value of h is measured by non-destructive testing methods such as CT), and then the residual compressive strength σ of the CFRTP with delamination damage is calculated. c , the formula is as follows:

[0051]

[0052] Where k is unitless; σ b The unit of is MPa; the unit of d and h is mm;

[0053] When the environment is at normal temperature (temperature is 20-30°C, relative humidity is 40%-60%RH), k=1;

[0054] When the environment is a high temperature environment (temperature is 60-200°C, relative humidity is 40%-60%RH), T is the ambient temperature, in °C, and its value is measured by a thermometer; T0 is the change parameter of the elastic modulus of CFRTP at high temperature, with a value of 100, in °C; E T E is the elastic modulus of the undamaged CFRTP at ambient temperature, in MPa, and is measured by the DMA (dynamic mechanical properties analysis) method; R is the elastic modulus of the undamaged CFRTP at room temperature (i.e., 25°C), in MPa, and its value is measured by the DMA (dynamic mechanical properties analysis) method;

[0055] When the environment is hot and humid (temperature is 40-100°C, relative humidity is 65%-100%RH), t is the value of the damp heat aging time in h, and its value is obtained by timing with a timer. For example, if the damp heat aging time is 1 h, then t is 1; e is the base of the natural logarithm function (e = 2.71828183); T is the ambient temperature in °C, and its value is obtained by measuring with a thermometer; T g T is the glass transition temperature of CFRTP, in °C, and its value is measured by DSC (differential scanning calorimetry) and DMA method; s is the parameter affecting the performance of CFRTP under the humid and hot environment, which is 10 and the unit is ℃; a and b are the unknown constants related to the humid and hot conditions, and their values ​​are obtained by dividing the σ under the specific humid and hot environment by c The experimental value of σ b The experimental values ​​of d, h, t, T, Tg 、T s Substitute it into the following formula to obtain;

[0056]

[0057] In order to verify the accuracy of the prediction method of the present invention for the compressive residual strength of CFRTP with delamination damage, the present invention uses the room temperature compressive residual strength prediction model of CFRTP with delamination damage of different depths to calculate the compressive residual strength of CF / PA6, CF / PPS and CF / PEEK composite materials with delamination damage of different depths (composite material thickness 4mm) (delamination at the geometric center of the material, diameter 50mm), and the results are shown in Tables 1, 2 and 3. It can be seen from the table that the calculated error values ​​are all less than 8%, proving that the room temperature compressive residual strength prediction model derived in this paper is universal for CFRTP with delamination damage.

[0058] Table 1 Comparison of measured and calculated residual strength of CF / PPS composites with different depths of delamination damage at room temperature

[0059] Table 2 Comparison of measured and calculated residual strength of CF / PA6 composites with different depths of delamination damage at room temperature

[0060] Table 3 Comparison of measured and calculated residual strength of CF / PEEK composites with different depths of delamination damage at room temperature

[0061] The room temperature compressive strength and elastic modulus (E) of the undamaged CF / PA6, CF / PPS and CF / PEEK composites measured in the experiment under high temperature environment (as shown in Table 4) were substituted into formula (5) to calculate the compressive residual strength of the CF / PA6, CF / PPS and CF / PEEK composites with delamination damage (delamination at the geometric center of the material, between the 5 / 6 layers, with a diameter of 50 mm) under high temperature. The results are shown in Tables 5, 6 and 7. It can be seen that the high temperature compressive residual strength of the CFRTP with delamination damage calculated by the model has an error of less than 10% with the actual measured value obtained by the experiment, which verifies the accuracy of the prediction model.

[0062] Table 4 Calculation parameters of residual strength of CF / PA6, CF / PPS and CF / PEEK composites with delamination damage at high temperature

[0063] Table 5 Comparison of measured and calculated values ​​of residual strength of CF / PA6 composites with delamination damage at high temperature

[0064] Table 6 Comparison between measured and calculated values ​​of residual strength of CF / PPS composites with delamination damage at high temperature

[0065] Table 7 Comparison of measured and calculated values ​​of residual strength of CF / PEEK composites with delamination damage at high temperature

[0066] The compressive residual strength of CF / PA6, CF / PPS and CF / PEEK composite materials with delamination damage (delamination at the geometric center of the material, between the 5 / 6 layers, with a diameter of 50 mm) after 112 hours of wet heat aging (100°C / 100% RH) was calculated. The values ​​of a and b were calculated to be -0.002 and 1, respectively. The relationship between the compressive strength and the wet heat time under this wet heat condition is: The results are shown in Table 8. It can be seen that the errors are all less than 7%, which verifies the reliability of the prediction model.

[0067] Table 8 Comparison of measured and calculated values ​​of compressive residual strength after hygrothermal aging of CFRTP with delamination damage

[0068] The present invention also provides a method for repairing CFRTP with delamination damage, that is, application of the above-mentioned method for predicting the compressive residual strength of CFRTP with delamination damage, comprising the following steps:

[0069] (i) using the prediction method for compressive residual strength of CFRTP with delamination damage as described in any one of the above items to obtain the compressive residual strength of CFRTP with delamination damage;

[0070] (ii) determining whether the delamination damage reaches the damage tolerance of CFRTP, if yes, proceeding to step (iii); otherwise, proceeding to step (iv);

[0071] (iii) repairing the delamination beyond the damage tolerance by using a resin injection method, and returning to step (i);

[0072] (iv) Continue to use CFRTP.

Claims

1. A method for predicting the compressive residual strength of CFRTP with delamination damage, characterized in that: Determine the environment-related coefficient k and the damage-free CFRTP compressive strength σ b , the delamination damage depth d, and the total thickness h of the CFRTP with delamination damage are substituted into the formula to calculate the compressive residual strength σ of the CFRTP with delamination damage c , the formula is as follows: Where k is unitless; σ b The unit of is MPa; the unit of d and h is mm; When the environment is at normal temperature, k = 1; When the environment is high temperature, T is the ambient temperature, in °C; T0 is the change parameter of the elastic modulus of CFRTP at high temperature, with a value of 100, in °C; E T is the elastic modulus of the undamaged CFRTP at ambient temperature, in MPa; E R is the elastic modulus of undamaged CFRTP at room temperature, in MPa; When the environment is hot and humid, t is the value of the wet heat aging time in h; e is the base of the natural logarithm function; T is the ambient temperature in °C; T g is the glass transition temperature of CFRTP, in °C; T s is the parameter affecting the performance of CFRTP under the humid and hot environment, which is 10 and the unit is ℃; a and b are the unknown constants related to the humid and hot conditions, and their values ​​are obtained by dividing the σ under the specific humid and hot environment by c The experimental value of σ b The experimental values ​​of d, h, t, T, T g , T s Substitute it into the following formula to obtain; The temperature of the normal temperature environment is 20-30°C, and the relative humidity is 40%-60% RH; the temperature of the high temperature environment is 60-200°C, and the relative humidity is 40%-60% RH; the temperature of the humid and hot environment is 40-100°C, and the relative humidity is 65%-100% RH.

2. The method for predicting the compressive residual strength of CFRTP with delamination damage according to claim 1, characterized in that: σ b The value of is measured by ASTM D 3410-03, a standard test method for compressive properties of polymer matrix composites.

3. The method for predicting the compressive residual strength of CFRTP with delamination damage according to claim 1, characterized in that: The value of d is measured using a vernier caliper.

4. The method for predicting the compressive residual strength of CFRTP with delamination damage according to claim 1, characterized in that: The value of h is obtained by non-destructive testing.

5. A method for repairing CFRTP with delamination damage, characterized in that: The following steps are involved: (i) obtaining the compressive residual strength of the CFRTP with delamination damage by using the prediction method of the compressive residual strength of the CFRTP with delamination damage as described in any one of claims 1 to 4; (ii) determining whether the delamination damage reaches the damage tolerance of CFRTP, if yes, proceeding to step (iii); otherwise, proceeding to step (iv); (iii) repairing the delamination that exceeds the damage tolerance and returning to step (i); (iv) Continue to use CFRTP.

6. A method for repairing CFRTP with delamination damage according to claim 5, characterized in that: The repair is performed by injection resin method.