Preparation method and application of tris(2-cyanoethyl)phosphite
By preparing tri(2-cyanoethyl)phosphite as the electrolyte additive for lithium-ion batteries, the problems of insufficient types of existing electrolyte additives and complex processes have been solved, the high temperature and circulation performance of lithium-ion batteries have been improved, and the high temperature and circulation performance of lithium-ion batteries have been achieved. Products with cyano content and high-efficiency process.
Patent Information
- Application Number
- CN202210814870.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-07-12
AI Technical Summary
The existing lithium-ion battery electrolyte additives are insufficient, which is difficult to meet the needs of high voltage and high temperature performance, and the process is complex and the product has a low cyano content.
Using the preparation method of tri(2-cyanoethyl)phosphite, by dropwise addition of phosphorus trichloride solution with 3-hydroxypropionitrile and organic alkali metal salt under protective gas conditions, combined with two-step temperature control and The organic base catalyst prepared a tris(2-cyanoethyl)phosphite with a high cyano content as an additive for electrolyte of high voltage lithium ion battery.
It improves the high-temperature performance and cycling performance of lithium-ion batteries, has simple and feasible process, low energy consumption, high yield, is suitable for industrial promotion and application, and the product purity reaches more than 97%.
Smart Images

Figure BDA0003741952430000031 
Figure BDA0003741952430000071 
Figure BDA0003741952430000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery electrolytes and relates to a preparation method and application of cyanophosphite, in particular to a preparation method and application of tris(2-cyanoethyl)phosphite. Background Art
[0002] Lithium-ion battery is a secondary battery (rechargeable battery) that mainly relies on the movement of lithium ions between the positive and negative electrodes to work. + Insertion and deinsertion back and forth between the two electrodes: During charging, Li + It is deintercalated from the positive electrode and embedded into the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state; the opposite is true during discharge. Batteries generally use materials containing lithium as electrodes and are the representative of modern high-performance batteries. Lithium-ion batteries usually include positive electrodes, negative electrodes, diaphragms, electrolytes and shells. They have the advantages of high operating voltage, high specific energy, long cycle life, light weight, low self-discharge, no memory effect and high performance-price ratio. They have become the main choice of rechargeable power sources in high-power electric vehicles, artificial satellites, aerospace and other fields.
[0003] Lithium-ion batteries have the advantages of high energy density, high operating voltage, long cycle life, no memory effect, and low environmental pollution. They have been widely used in 3C, energy storage, power and other fields. However, with the development requirements of miniaturization of 3C products and long driving range of new energy vehicles, higher requirements are placed on the overall performance of lithium-ion batteries, especially in terms of energy density and cycle performance. Under the existing positive and negative electrode system, increasing the battery charging voltage is the most effective way to increase the battery energy density, but this will bring great challenges to the lithium-ion battery electrolyte.
[0004] Phosphate compounds (such as tris(trimethylsilyl)phosphate, lithium difluorophosphate, lithium difluorobis(oxalate phosphate, etc.) and nitrile compounds (such as adiponitrile, succinonitrile, 1,3,6-hexanetrinitrile, 1,2-bis(2-cyanoethoxy)ethane, etc.), as common additives for lithium-ion electrolytes, have a significant effect in improving the high voltage performance, high temperature performance and cycle performance of lithium-ion batteries. However, as the downstream application industry gradually increases the performance requirements of lithium-ion batteries, further developing more types of lithium-ion electrolyte additives has become one of the urgent problems to be solved by many front-line researchers and scientific research enterprises in this field. Summary of the invention
[0005] In view of this, the present invention provides a preparation method and application of cyanophosphite, in particular a preparation method of tris(2-cyanoethyl)phosphite. The present invention provides a cyanophosphite, namely tris(2-cyanoethyl)phosphite, with a simple and feasible preparation process. The product can be used as an electrolyte additive for high-voltage lithium-ion batteries to improve the high temperature performance and cycle performance of the battery.
[0006] The present invention provides a method for preparing cyanophosphite, comprising the following steps:
[0007] 1) mixing 3-hydroxypropionitrile, a hydrogen chloride chelating agent and an organic alkali metal salt to obtain a mixture;
[0008] 2) under protective gas conditions, at a first temperature, adding a phosphorus trichloride organic solution to the system solution obtained in the above step to react, and continuing the reaction at a second temperature to obtain a cyanophosphite;
[0009] The cyanophosphite includes tris(2-cyanoethyl)phosphite.
[0010] Preferably, the hydrogen chloride chelating agent includes one or more of triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine and pyridine;
[0011] The organic alkali metal salt includes one or more of sodium hydrogen, sodium methoxide, sodium ethoxide, potassium ethoxide, sodium methoxide, potassium tert-butoxide, n-butyl lithium and lithium diisopropylamide;
[0012] The solvent in the phosphorus trichloride organic solution includes one or more of toluene, n-hexane, petroleum ether, diethyl ether, tert-methyl butyl ether, dichloromethane and dichloroethane.
[0013] Preferably, the molar ratio of the hydrogen chloride chelating agent to phosphorus trichloride is (3-6):1;
[0014] The molar ratio of 3-hydroxypropionitrile to phosphorus trichloride is (3-10):1;
[0015] The mass ratio of the organic alkali metal salt to the hydrogen chloride chelating agent is (0.01-1):100;
[0016] In the phosphorus trichloride organic solution, the volume ratio of the solvent to phosphorus trichloride is (1-10):1.
[0017] Preferably, the first temperature is -40 to 10°C;
[0018] The dropping rate is 5-20 ml / h.
[0019] Preferably, the temperature of the continued reaction is 30 to 100°C;
[0020] The continued reaction time is 1 to 20 hours;
[0021] After the continued reaction, a purification step is also included;
[0022] The purification step comprises: mixing the crude reaction product obtained after the reaction is continued with an alkali solution, adding an organic solvent and mixing again, separating the organic phase, and then removing the organic solvent to obtain cyanophosphite.
[0023] Preferably, the alkali solution includes one or more of NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2 and NaHCO3;
[0024] The mass concentration of the alkali solution is 1% to 20%;
[0025] The organic solvent includes one or more of dichloromethane, dichloroethane, benzene, toluene, octane, petroleum ether, tridecane, octacosane, carbon disulfide, carbon tetrachloride, ethane and cyclohexane.
[0026] Preferably, the cyanophosphite is tris(2-cyanoethyl)phosphite;
[0027] The cyanophosphite has a structure as shown in formula (I):
[0028]
[0029] Preferably, the cyanophosphite is a lithium ion battery additive;
[0030] The lithium ion battery includes a lithium ion battery electrolyte;
[0031] The mass content of the cyanophosphite in the lithium ion battery electrolyte is 0.1% to 5%.
[0032] The present invention also provides the use of cyanophosphite prepared by the preparation method described in any one of the above technical solutions in lithium ion batteries.
[0033] Preferably, the lithium-ion battery comprises a high-voltage lithium-ion battery;
[0034] The lithium-ion battery is specifically an electrolyte of a lithium-ion battery;
[0035] The cyanophosphite is used as an additive for lithium ion battery electrolyte.
[0036] The present invention provides a method for preparing cyanophosphite, comprising the following steps: first, 3-hydroxypropionitrile, a hydrogen chloride chelating agent and an organic alkali metal salt are mixed to obtain a mixture; then, under protective gas conditions, at a first temperature, a phosphorus trichloride organic solution is added dropwise to the system solution obtained in the above step to react, and at a second temperature, the reaction is continued to obtain cyanophosphite; the cyanophosphite includes tris(2-cyanoethyl)phosphite. Compared with the prior art, the present invention aims at the problem that the types of existing lithium ion electrolyte additives need to be further developed, starting from the direction of phosphite compounds, although there are products and methods for preparing 2-cyanoethyl dichlorophosphate and 2-cyanoethyl phosphoric acid in the existing process, and there is also a technical solution disclosed, which is to prepare a di(propionitrile)phosphoric acid compound by 3-hydroxypropionitrile and hypophosphorous acid, react with an iodoalkane compound under the dual action of a catalyst and a base, and synthesize a dicyanophosphate compound, which is a technical solution that plays a beneficial effect in lithium ion batteries as an electrolyte additive. However, there are problems that the process is relatively complicated and the cyano content of the product needs to be improved. The present invention believes that both cyano (-CN) and phosphate groups are effective structures of cyanophosphate additives. In theory, the higher the proportion of this effective structure, the better the beneficial effect as an additive. However, due to steric hindrance effects and the difficulty in separating organic matter with different degrees of substitution, the number of cyano groups in cyanophosphate compounds is limited.
[0037] Based on this, the present invention creatively obtains tris(2-cyanoethyl)phosphite having a structure of formula (I) and a preparation method thereof. The cyanophosphite compound prepared by the present invention is tris(2-cyanoethyl)phosphite, which contains three cyano (-CN) groups and a phosphoric acid group in its molecular structure. The cyanophosphite compound has a novel structure and can be used as an electrolyte additive for high-voltage lithium-ion batteries to improve the high temperature performance and cycle performance of the battery.
[0038] Moreover, the preparation method of tris(2-cyanoethyl)phosphite provided by the present invention and the specific separation and purification step of tris(2-cyanoethyl)phosphite particularly adopt the dual effects of two-step temperature control and organic base catalyst to promote the forward reaction of 3-hydroxypropionitrile and phosphorus trichloride, and then separate to obtain tris(2-cyanoethyl)phosphite. The preparation method provided by the present invention has simple and feasible process, low energy consumption, high yield, and is particularly suitable for industrial promotion and application.
[0039] The experimental results show that the target structure product is synthesized by the synthesis method provided by the present invention, and the purity reaches more than 97%. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the infrared spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention;
[0041] Figure 2 This is the C NMR spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention;
[0042] Figure 3 To calculate the nuclear magnetic chemical shift of C in tris(2-cyanoethyl)phosphite using ChemDraw software;
[0043] Figure 4 This is the H NMR spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention;
[0044] Figure 5 To calculate the nuclear magnetic chemical shift of H in tris(2-cyanoethyl)phosphite using ChemDraw software;
[0045] Figure 6 This is the NMR P spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0046] In order to further understand the present invention, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0048] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity in the field of lithium-ion batteries.
[0049] The present invention provides a method for preparing cyanophosphite, comprising the following steps:
[0050] 1) mixing 3-hydroxypropionitrile, a hydrogen chloride chelating agent and an organic alkali metal salt to obtain a mixture;
[0051] 2) under protective gas conditions, at a first temperature, adding a phosphorus trichloride organic solution to the system solution obtained in the above step to react, and continuing the reaction at a second temperature to obtain a cyanophosphite;
[0052] The cyanophosphite includes tris(2-cyanoethyl)phosphite.
[0053] The invention firstly mixes 3-hydroxypropionitrile, a hydrogen chloride chelating agent and an organic alkali metal salt to obtain a mixture.
[0054] In the present invention, the hydrogen chloride chelating agent preferably includes one or more of triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine and pyridine, more preferably triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine or pyridine.
[0055] In the present invention, the organic alkali metal salt preferably includes one or more of sodium hydrogen, sodium methoxide, sodium ethoxide, potassium ethoxide, sodium methoxide, potassium tert-butoxide, n-butyl lithium and lithium diisopropylamide, and more preferably includes sodium hydrogen, sodium methoxide, sodium ethoxide, potassium ethoxide, sodium methoxide, potassium tert-butoxide, n-butyl lithium or lithium diisopropylamide.
[0056] The present invention then adds a phosphorus trichloride organic solution dropwise to the system solution obtained in the above step under protective gas conditions at a first temperature for reaction, and continues the reaction at a second temperature to obtain cyanophosphite;
[0057] The cyanophosphite includes tris(2-cyanoethyl)phosphite.
[0058] In the present invention, the solvent in the phosphorus trichloride organic solution preferably includes one or more of toluene, n-hexane, petroleum ether, ethyl ether, tert-methyl butyl ether, dichloromethane and dichloroethane, and more preferably toluene, n-hexane, petroleum ether, ethyl ether, tert-methyl butyl ether, dichloromethane or dichloroethane.
[0059] In the present invention, the molar ratio of the hydrogen chloride chelating agent to phosphorus trichloride is preferably (3-6):1, more preferably (3.5-5.5):1, more preferably (4-5):1, and specifically (3-4):1.
[0060] In the present invention, the molar ratio of 3-hydroxypropionitrile to phosphorus trichloride is preferably (3-10): 1, more preferably (4-9): 1, more preferably (5-8): 1, more preferably (6-7): 1, and specifically (3-5): 1. Specifically, the 3-hydroxypropionitrile of the present invention preferably uses an excess of 3-hydroxypropionitrile.
[0061] In the present invention, the mass ratio of the organic alkali metal salt to the hydrogen chloride chelating agent is preferably (0.01-1):100, more preferably (0.1-0.9):100, more preferably (0.2-0.8):100, more preferably (0.3-0.7):100, more preferably (0.4-0.6):100.
[0062] In the present invention, in the phosphorus trichloride organic solution, the volume ratio of the solvent to phosphorus trichloride is preferably (1-10):1, more preferably (3-8):1, more preferably (5-6):1, and specifically (2-3):1.
[0063] In the present invention, the first temperature is preferably -40 to 10°C, more preferably -30 to 5°C, more preferably -30 to -0°C, more preferably -20 to -5°C, and specifically -30 to -5°C.
[0064] In the present invention, the dropping rate is preferably 5 to 20 ml / h, more preferably 8 to 17 ml / h, more preferably 11 to 14 ml / h, and specifically 10 to 15 ml / h.
[0065] In the present invention, the temperature of the continued reaction is preferably 30-100°C, more preferably 50-85°C, more preferably 60-80°C, more preferably 65-70°C, and specifically 50-80°C.
[0066] In the present invention, the time for the continued reaction is preferably 1 to 20 hours, more preferably 5 to 16 hours, more preferably 9 to 12 hours, and specifically 2 to 15 hours.
[0067] In the present invention, after the continued reaction, a purification step is preferably included.
[0068] In the present invention, the purification step preferably includes: mixing the crude reaction product obtained after the reaction is continued with an alkali solution, adding an organic solvent and mixing again, separating the organic phase, and then removing the organic solvent to obtain cyanophosphite.
[0069] In the present invention, the alkali solution preferably includes one or more of NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2 and NaHCO3, and more preferably NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2 or NaHCO3.
[0070] In the present invention, the mass concentration of the alkali solution is preferably 1% to 20%, more preferably 5% to 16%, more preferably 9% to 12%, and specifically can be 1% to 10%.
[0071] In the present invention, the organic solvent preferably includes one or more of dichloromethane, ethylene dichloride, benzene, toluene, octane, petroleum ether, tridecane, octacosane, carbon disulfide, carbon tetrachloride, ethane and cyclohexane, more preferably dichloromethane, ethylene dichloride, benzene, toluene, octane, petroleum ether, tridecane, octacosane, carbon disulfide, carbon tetrachloride, ethane or cyclohexane.
[0072] In the present invention, the cyanophosphite is preferably tris(2-cyanoethyl)phosphite;
[0073] The cyanophosphite preferably has a structure as shown in formula (I):
[0074]
[0075] In the present invention, the cyanophosphite is preferably a lithium ion battery additive.
[0076] In the present invention, the lithium ion battery preferably includes a lithium ion battery electrolyte.
[0077] In the present invention, the mass content of the cyanophosphite in the lithium ion battery electrolyte is preferably 0.1% to 5%, more preferably 0.5% to 4%, and more preferably 1% to 3%.
[0078] The present invention is to complete and refine the overall preparation process, better ensure the structure of cyanophosphite, and improve the purity and yield of the product. The preparation method of the cyanophosphite can specifically be the following steps:
[0079] 1) Add 3-hydroxypropionitrile, an organic hydrochloric acid chelating agent and a small amount of an organic alkali metal salt mixture into a four-necked flask;
[0080] 2) introducing an inert gas into the reaction vessel of step 1);
[0081] 3) adding a mixed solution of phosphorus trichloride and an organic diluent solvent dropwise to step 2) under the temperature condition of section I, and controlling the dropping rate and the reaction temperature;
[0082] 4) After the dropwise addition is completed, the reaction is continued for 1 to 20 hours under the temperature conditions of stage II;
[0083] 5) The crude product after the reaction in step 4) is added into alkaline water to dissolve, and an organic solvent is added and stirred thoroughly, and then the organic phase is separated using a separatory funnel and the organic solvent is removed by vacuum distillation to obtain pure tri(2-cyanoethyl)phosphite.
[0084] Specifically, the hydrogen chloride chelating agent in step 1) is selected from one or a mixture of two or more of the following substances: triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine, and pyridine. The molar ratio of the hydrogen chloride chelating agent to phosphorus trichloride is 3:1 to 6:1, preferably 3:1 to 4:1.
[0085] Specifically, the organic alkali metal salt in step 1) is selected from one or a mixture of two or more of the following substances: sodium hydrogen hydrate, sodium methoxide, sodium ethoxide, potassium ethoxide, sodium methoxide, potassium tert-butoxide, n-butyl lithium, lithium diisopropylamide. The mass ratio of the organic metal base to the hydrogen chloride chelating agent is 0.01% to 1%;
[0086] Specifically, the inert gas in step 2) is N2, Ar, He, etc., preferably N2.
[0087] Specifically, in step 3), the molar ratio of 3-hydroxypropionitrile to phosphorus trichloride is 3:1 to 10:1, preferably 3:1 to 5:1.
[0088] Specifically, the organic solvent in step 3) is one or a mixture of two or more selected from the following substances: toluene, n-hexane, petroleum ether, ethyl ether, tert-methyl butyl ether, dichloromethane, dichloroethane, ethyl acetate. The volume ratio of the diluent to phosphorus trichloride is 1:1 to 10:1, preferably 2:1 to 3:1, and the dripping rate is 5 to 20 ml / h, preferably 10 to 15 ml / h;
[0089] Specifically, the temperature of the low-temperature reaction of the stage I reaction in step 3) is -40°C to 10°C, preferably -30°C to -0°C.
[0090] Specifically, the reaction temperature of stage II in step 4) is 30°C to 100°C, preferably 50 to 80°C, and the reaction time is 1 to 20 hours, preferably 2 to 15 hours.
[0091] Specifically, the alkaline water in step 5) is one or a mixture of two or more selected from the following substances: NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2, NaHCO3, etc. The concentration is 1%-20%, preferably 1%-10%.
[0092] Specifically, the organic solvent in step 5) is dichloromethane, ethylene dichloride, benzene, toluene, octane, petroleum ether, tridecane, octacosane, carbon disulfide, carbon tetrachloride, ethane, or cyclohexane.
[0093] The present invention provides a method for preparing the above compound, which comprises: under the protection of an inert gas, contacting 3-hydroxypropionitrile with phosphorus trichloride, and causing a substitution reaction between OH containing a cyano group and Cl in the phosphorus trichloride to obtain tris(2-cyanoethyl)phosphite and the above compound.
[0094] In the present invention, in order to obtain the above-mentioned compound, phosphorus trichloride is added dropwise to 3-hydroxypropionitrile. Relative to phosphorus trichloride, an excess of 3-hydroxypropionitrile can provide sufficient reaction raw materials for the reaction system to generate more tris(2-cyanoethyl)phosphite, which can further improve the yield of the product compound.
[0095] In the present invention, in order to obtain the above-mentioned compound, the phosphorus trichloride is diluted with an organic solution to control the reaction rate so that the reaction is more complete and the yield of the product compound can be further improved.
[0096] In the present invention, in order to obtain the above-mentioned compound, the selection of an organic alkali metal salt can promote the reaction, make the reaction mild, and further improve the product yield and product purity.
[0097] In the present invention, in order to obtain the above-mentioned compound, an organic base is selected as a hydrogen chloride chelating agent, and the organic base is triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine, pyridine, and the molar ratio of hydrogen chloride chelating agent to phosphorus trichloride is 3:1 to 6:1, preferably 3:1 to 4:1, which can further improve the yield of the product compound.
[0098] In the present invention, in order to obtain the above-mentioned compound, the dropwise addition reaction is carried out at the temperature of stage II after completion, the purpose of which is to provide conditions for overcoming the steric hindrance of the tri-substitution reaction and to increase the yield of the product compound.
[0099] In the present invention, in order to obtain the above-mentioned high-purity compound, alkaline water is used to dissolve the crude product and then an organic solvent is added for extraction. The di(2-cyanoethyl)phosphorous acid and cyanoethylphosphoric acid contain Cl and are more water-friendly. At the same time, alkaline water can neutralize the HCl generated by the reaction, thereby inhibiting the hydrolysis of tri(2-cyanoethyl)phosphite.
[0100] Specifically, the alkaline water is one or a mixture of two or more selected from the following substances: NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2, NaHCO3, etc., and its concentration is 1% to 20%, preferably 1% to 10%; its organic extractant can use at least one of dichloromethane, dichloroethane, chloroform, and ethyl acetate as the extractant, and the obtained product is purified by the organic phase to obtain high-purity tris(2-cyanoethyl)phosphite.
[0101] The present invention also provides the use of cyanophosphite prepared by the preparation method described in any one of the above technical solutions in lithium ion batteries.
[0102] In the present invention, the lithium ion battery preferably includes a high voltage lithium ion battery.
[0103] In the present invention, the lithium ion battery is preferably specifically an electrolyte of a lithium ion battery.
[0104] In the present invention, the cyanophosphite is preferably used as an additive for lithium ion battery electrolyte.
[0105] The above steps of the present invention provide a preparation method of tris(2-cyanoethyl)phosphite, tris(2-cyanoethyl)phosphite and applications. The tris(2-cyanoethyl)phosphite prepared by the present invention contains three cyano (-CN) groups and a phosphoric acid group in its molecular structure. The cyanophosphite compound has a novel structure and can be used as an electrolyte additive for high-voltage lithium-ion batteries to improve the high temperature performance and cycle performance of the battery.
[0106] Moreover, the preparation method of tris(2-cyanoethyl)phosphite provided by the present invention and the specific separation and purification step of tris(2-cyanoethyl)phosphite particularly adopt the dual effects of two-step temperature control and organic base catalyst to promote the forward reaction of 3-hydroxypropionitrile and phosphorus trichloride, and then separate to obtain tris(2-cyanoethyl)phosphite. The preparation method provided by the present invention has simple and feasible process, low energy consumption, high yield, and is particularly suitable for industrial promotion and application.
[0107] The experimental results show that the target structure product is synthesized by the synthesis method provided by the invention, and the purity reaches more than 97%.
[0108] In order to further illustrate the present invention, the preparation method and application of a cyanophosphite provided by the present invention are described in detail below in combination with examples. However, it should be understood that these examples are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following examples.
[0109] The reagents used in the following examples of the present invention are all commercially available products.
[0110] Example 1
[0111]
[0112] (1) Add 0.4 mol of anhydrous 3-hydroxypropionitrile, 0.3 mol of anhydrous triethylamine and 0.303 g of a mixed solution of sodium ethoxide into a four-necked flask, and control the reaction temperature to be below -30°C;
[0113] (2) N2 was introduced into the four-necked flask to replace the air in the reaction vessel.
[0114] (3) Mix 13.73 g of 0.1 mol of phosphorus trichloride and 100 ml of xylene and place in a constant pressure dropping funnel;
[0115] (4) adding the mixed solution of step (2) dropwise to the mixed solution of step (1), with the dropping rate controlled at 10 ml / h;
[0116] (5) After the addition is complete, the reaction is carried out at 65°C for 15 h;
[0117] (6) After the reaction, 100 ml of xylene was added to the reaction solution and triethylamine hydrochloride was filtered out;
[0118] (7) A 3% NaOH aqueous solution was added to the filtered filtrate and stirred for 30 min. The mixture was allowed to stand for separation. After rotary separation, xylene was removed from the organic phase solution to obtain pure tri(2-cyanoethyl)phosphite with a yield of 81.75%. The product content was measured by gas chromatography to be 97.3%.
[0119] The tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention was characterized and simulated.
[0120] See also Figure 1 , Figure 1 This is the infrared spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention.
[0121] See also Figure 2 , Figure 2 This is the C NMR spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention.
[0122] See also Figure 3 , Figure 3 The ChemDraw software was used to calculate the nuclear magnetic chemical shift of C in tris(2-cyanoethyl)phosphite.
[0123] See also Figure 4 , Figure 4 This is the H NMR spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention.
[0124] See also Figure 5 , Figure 5 The ChemDraw software was used to calculate the nuclear magnetic chemical shift of H in tris(2-cyanoethyl)phosphite.
[0125] See also Figure 6 , Figure 6 This is the NMR P spectrum of tris(2-cyanoethyl)phosphite prepared in Example 1 of the present invention.
[0126] from Figure 1 to Figure 6 It can be seen that the tris(2-cyanoethyl)phosphite prepared by the present invention.
[0127] like Figure 1 The infrared spectrum of the product prepared by the patent of this invention shows that 1024cm -1 and 977cm -1 It is the characteristic peak of POC stretching vibration absorption, 2260-2210cm -1 The absorption characteristic peak of -CN is 3000-2800cm -1 The absorption peak between -CH2 absorption characteristic peak. Figure 2 The nuclear magnetic resonance C spectrum of the product prepared by the present invention shows that the chemical shifts corresponding to the nuclear magnetic peaks are 20.46ppm, 57.76 and 117.59ppm respectively. Figure 3 The chemical shift of C in tris(2-cyanoethyl)phosphite calculated by ChemDraw software is consistent with that shown. Figure 4 The chemical shifts corresponding to the H NMR spectrum of the patented product are 2.65-2.68 and 4.03-4.08, which are consistent with Figure 5 The chemical shift of H in tri(2-cyanoethyl)phosphite was simulated and calculated using ChemDraw software and the results are consistent.
[0128] Example 2
[0129] (1) Add 0.3 mol of anhydrous 3-hydroxypropionitrile, 0.3 mol of anhydrous triethylamine and 0.015 g of a mixed solution of sodium ethoxide into a four-necked flask, and control the reaction temperature to be below -15°C;
[0130] (2) introducing N2 into a four-necked flask to displace the air in the reaction vessel;
[0131] (3) Mix 13.73 g of 0.1 mol of phosphorus trichloride and 100 ml of xylene and place in a constant pressure dropping funnel;
[0132] (4) adding the mixed solution of step (2) dropwise to the mixed solution of step (1), with the dropping rate controlled at 10 ml / h;
[0133] (5) After the addition is complete, the reaction is carried out at 70°C for 5 h;
[0134] (6) After the reaction, 100 ml of xylene was added to the reaction solution and triethylamine hydrochloride was filtered out;
[0135] (7) A 10% NaOH aqueous solution was added to the filtered filtrate, and the mixture was stirred for 30 min and then allowed to stand for separation. After rotary separation, xylene was removed from the organic phase solution to obtain pure tri(2-cyanoethyl)phosphite with a yield of 82.5%. The product content was measured by gas chromatography to be 97.8%.
[0136] Example 3
[0137] (1) Add 3 mol of anhydrous 3-hydroxypropionitrile, 3 mol of anhydrous triethylamine and 3.03 g of a mixed solution of sodium ethoxide into a four-necked flask, and control the reaction temperature to be below -30°C;
[0138] (2) introducing N2 into a four-necked flask to displace the air in the reaction vessel;
[0139] (3) Mix 137.33 g of 1 mol of phosphorus trichloride and 1000 ml of xylene and place in a constant pressure dropping funnel;
[0140] (4) adding the mixed solution of step (2) dropwise to the mixed solution of step (1), with the dropping rate controlled at 10 ml / h;
[0141] (5) After the addition is complete, the reaction is carried out at 65°C for 15 h;
[0142] (6) After the reaction, 1000 ml of xylene was added to the reaction solution and triethylamine hydrochloride was filtered out;
[0143] (7) Add 5% NaOH aqueous solution to the filtered filtrate and stir for 30 minutes, then stand for separation. After rotary separation, remove xylene from the organic phase solution to obtain pure tri(2-cyanoethyl)phosphite with a yield of 81.5%. The product content was measured by gas chromatography to be 97.1%.
[0144] The preparation method and application of tris(2-cyanoethyl)phosphite provided by the present invention are introduced in detail above. The principle and implementation mode of the present invention are described by using specific examples herein. The description of the above embodiments is only used to help understand the method and core idea of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in the technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims, and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the textual expression of the claims, or if they include equivalent structural elements that are not substantially different from the textual expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for preparing a high-yield cyanophosphite, characterized in that: The following steps are involved: 1) mixing 3-hydroxypropionitrile, a hydrogen chloride chelating agent and an organic alkali metal salt to obtain a mixture; The hydrogen chloride chelating agent is one or more of triethylamine, diethylamine, ethylenediamine, dipropylamine, tripropylamine, propylenediamine, n-butylamine and pyridine; The organic alkali metal salt is one or more of sodium hydrogen, sodium methoxide, sodium ethoxide, potassium ethoxide, sodium methoxide, potassium tert-butoxide, n-butyl lithium and lithium diisopropylamide; The molar ratio of the hydrogen chloride chelating agent to phosphorus trichloride is (3-6):1; The molar ratio of 3-hydroxypropionitrile to phosphorus trichloride is (3-10):1; The mass ratio of the organic alkali metal salt to the hydrogen chloride chelating agent is (0.01-1):100; 2) under protective gas conditions, at a first temperature, adding a phosphorus trichloride organic solution to the system solution obtained in the above step to react, and continuing the reaction at a second temperature to obtain a cyanophosphite; The first temperature is greater than or equal to -40°C to 0°C; The temperature of the continued reaction is 30 to 100° C. The cyanophosphite is tris(2-cyanoethyl)phosphite.
2. The preparation method according to claim 1, characterized in that: The solvent in the phosphorus trichloride organic solution is one or more of toluene, n-hexane, petroleum ether, ethyl ether, tert-methyl butyl ether, dichloromethane and dichloroethane.
3. The preparation method according to claim 1, characterized in that: In the phosphorus trichloride organic solution, the volume ratio of the solvent to phosphorus trichloride is (1-10):
1.
4. The preparation method according to claim 1, characterized in that: The dropping rate is 5-20 ml / h.
5. The preparation method according to claim 1, characterized in that: The continued reaction time is 1 to 20 hours; After the continued reaction, a purification step is also included; The purification step comprises: mixing the crude reaction product obtained after the reaction is continued with an alkali solution, adding an organic solvent and mixing again, separating the organic phase, and then removing the organic solvent to obtain cyanophosphite.
6. The preparation method according to claim 5, characterized in that: The alkali solution is one or more of NaOH, LiOH, KOH, Ba(OH)2, Ca(OH)2, Na(CO3)2 and NaHCO3; The mass concentration of the alkali solution is 1% to 20%; The organic solvent is one or more of dichloromethane, dichloroethane, benzene, toluene, octane, petroleum ether, tridecane, octacosane, carbon disulfide, carbon tetrachloride, ethane and cyclohexane.
7. The preparation method according to claim 1, characterized in that: The cyanophosphite has a structure as shown in formula (I):
8. The preparation method according to claim 1, characterized in that: The cyanophosphite is a lithium ion battery additive; The lithium ion battery includes a lithium ion battery electrolyte; The mass content of the cyanophosphite in the lithium ion battery electrolyte is 0.1% to 5%.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The cyanophosphite is a cyanophosphite used in lithium ion batteries.
10. The preparation method according to claim 9, characterized in that: The lithium-ion battery is a high-voltage lithium-ion battery; The lithium-ion battery is specifically an electrolyte of a lithium-ion battery; The cyanophosphite is used as an additive for lithium ion battery electrolyte.