A method for preparing fiber spinning solution by low-temperature dissolution

Through the combination of low-temperature swelling and high-concentration NMMO solution, the problems of high energy consumption and thermal degradation in the preparation of Lyocell fiber spinning dope are solved, the cellulose is fully swollen and the mechanical properties are improved, the formation of the gel layer is reduced, and the cost is saved energy consumption and increased cellulose permeability.

CN115044985BActive Publication Date: 2024-10-15SAIDELI (CHANGZHOU) FIBER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210716699.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-10-15
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

In the existing Lyocell fiber spinning dope preparation method, the high swelling temperature leads to high energy consumption, easy formation of gel layer, serious thermal degradation, and the direct dissolution method has high cost, great safety hazards, and poor dissolution effect.

Method used

Low molecular weight alcohol solvents, low molecular weight ether solvents and polymers are mixed with high-concentration NMMO solutions. After swelling at low temperature, the temperature is raised to above 75°C for dissolution. Stirring or vacuum conditions are used to prepare the fiber spinning stock solution, and the swelling temperature is controlled at 50℃~55℃, and remove organic matter by heating or vacuum to reduce energy consumption.

Benefits of technology

It can achieve full swelling of cellulose at low temperature, reduce thermal degradation, improve the mechanical properties of cellulose, save energy consumption, reduce the formation of gel layer, and improve the permeability and dissolution effect of cellulose.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing fiber spinning solution by low-temperature dissolution, comprising the following steps: S1) mixing one or more of a low molecular weight alcohol solvent, a low molecular weight ether solvent and a polymer with a high concentration NMMO solution to obtain a mixed solution; S2) mixing the mixed solution with crushed pulp for swelling, and then vacuuming and heating to 75°C or above for dissolution to obtain a fiber spinning solution; the swelling temperature is less than or equal to 55°C. Compared with the prior art, the present invention performs swelling at a low temperature, is not easy to form an initial dissolution, is conducive to the full penetration and diffusion of the NMMO solution, and the swelling is more complete. At the same time, the added organic matter can increase the penetration of the solution to cellulose, further increasing the swelling effect; further, the added organic matter can be removed by heating, and the dissolution zone is reached in a short time, which saves energy consumption costs while greatly reducing the thermal degradation of cellulose, thereby improving the mechanical properties and strength of cellulose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber preparation, and in particular relates to a method for preparing fiber spinning solution by low-temperature dissolution. Background Art

[0002] Cellulose is the most abundant and widely distributed natural polymer on earth, and is an inexhaustible renewable resource in nature. Cellulose fiber has the advantages of high strength, good dyeability, good spinning performance and wide industrial applications. Therefore, the market demand for cellulose fiber has continued to increase in recent years.

[0003] Among them, Lyocell fiber is made from renewable resources such as cotton linter, trees, bamboo, etc., with NMMO as solvent, through dry-jet wet spinning. It is a cellulose fiber that has many excellent properties of both natural fibers and synthetic fibers, and the production process is green and environmentally friendly.

[0004] Lyocell fiber has the advantages of high strength, good dyeability, good spinning performance and wide industrial applications. Compared with viscose fiber, it has more outstanding performance, short process flow and green and pollution-free production process. Therefore, the market demand for Lyocell fiber has continued to increase in recent years.

[0005] At present, the preparation methods of Lyocell fiber spinning solution mainly include indirect dissolution method (wet method and dry method) and direct dissolution method.

[0006] Indirect dissolution method: Mix medium and low concentration NMMO aqueous solution with cellulose pulp, and after sufficient swelling, remove excess water through reduced pressure distillation to reach the dissolution range to complete dissolution. Medium and low concentration NMMO solution cannot dissolve cellulose, and excess water is conducive to the full swelling of cellulose molecules in the solvent, which is easy to form a uniform slurry. The indirect dissolution method can be divided into wet method and dry method. The wet method is to mix pulp with water to make pulp, then squeeze the pulp solution to remove water, and then mix it with NMMO after crushing, and swell in a storage tank to make NMMO and cellulose fully combine to form cellulose slurry. In the wet process, when the wet pulp is mixed with the NMMO solution, the NMMO concentration is about 80% to 84%. After swelling is completed, the slurry is transported to the reactor (such as a thin film evaporator) to dissolve to form a spinning solution, and the spinning solution is transported to the spinning machine to complete spinning. In the dry method, the pulp does not need to be mixed with water, crushed, or processed. It is directly mixed with the NMMO solution in the form of a pulp board. Compared with the wet method, the hydraulic pulping and pressing processes are omitted. The concentration of the NMMO solution required for dry pulp mixing is between 75% and 80%. After swelling is completed, the pulp porridge is transported to a reactor (such as a thin film evaporator) for dissolution to form a spinning solution, which is then transported to a spinning machine to complete spinning. The current dry method mainly uses medium-high concentration NMMO (75% to 80%) to stir and swell at 80 to 85°C. After swelling is complete, it is added to a vacuum stirring reactor and stirred at about 95°C to 105°C to vacuum evaporate water for 2 to 3 hours to prepare a transparent and uniform colloid in the dissolution range. However, this method has the following disadvantages: ① The swelling temperature is high and the energy consumption is large. ② The swelling temperature is high, and initial dissolution is easy to occur. A gel layer is formed on the surface of cellulose, which hinders the solvent from continuing to penetrate and diffuse into the interior of cellulose. The prepared colloid may contain some insoluble white cores. ③ The vacuum evaporation temperature is high, the energy consumption is large, cellulose, PG, NMMO, etc. are prone to thermal degradation, and the reaction time is long, the quality and performance of the subsequent glue solution and finished silk are reduced, and the color of the colloidal solution deepens, which increases the burden of the anionic and cationic resins for subsequent solvent recovery. ④ Simply directly lowering the swelling temperature, the NMMO solution is easy to crystallize and solidify, and the osmotic swelling speed slows down, and the swelling effect becomes worse.

[0007] Some people also use NMMO solid to directly add it into ethanol solution in the laboratory to prepare colloids with 1-3% cellulose content, which has the following disadvantages: ① The preparation cost of NMMO solid is too high; ② NMMO solid is dark in color, which has an adverse effect on the quality of subsequent finished silk, and will also increase the burden on anion and cation exchange resins in the solvent recovery workshop; ③ Too much ethanol is added, which increases the cost, and too high ethanol content poses a safety hazard in actual production: ④ The prepared colloid has a cellulose content of 1-3%, which is too low to be used in actual production.

[0008] Direct dissolution method: directly mix the high-concentration NMMO solution with dissolving ability with the crushed cellulose pulp under appropriate conditions, and dissolve it directly without swelling. This method does not need to remove water during the dissolution process, which simplifies the process. However, because cellulose will dissolve when it comes into contact with the high-concentration NMMO solution, the solvent molecules may not have penetrated into the interior of the cellulose, and the surface has already been initially dissolved, which is easy to form a "gel mass", which hinders the solvent from continuing to penetrate and diffuse into the interior of the cellulose. The prepared gel may contain some insoluble white cores. In order to overcome the shortcomings of the direct dissolution method, there are currently the following solutions: ① crush the cellulose raw material into extremely small particle size particles; ② use a supercooled liquid of NMMO / water solvent, the low temperature reduces the solvent's dissolving ability or loses its dissolving ability, and the cellulose is fully swelled and then heated to complete the dissolution. However, crushing into fluff is costly, and using fluffy cellulose as raw material in the workshop is prone to safety hazards. If larger particles are used as raw materials and complete dissolution is required, a large rotation speed or strong mechanical force is required to destroy them, which will affect the physical and chemical properties of the cellulose itself. Physically preparing a supercooled liquid with a high concentration of NMMO / water solvent requires a short-term temperature drop, which has high technical requirements and high costs, and is not suitable for workshop production. Chemical methods to prepare a supercooled liquid with a high concentration of NMMO / water solvent require the addition of polyvinyl alcohol, which has a high molecular weight and is a white solid. It needs to be heated and stirred to dissolve, and has a high viscosity, which will reduce the pulp to a certain extent. The penetration of NMMO during meal premixing reduces the solubility of cellulose in the NMMO solution. After the addition of polyvinyl alcohol, due to its high viscosity and many molecular chains, it is easy to produce molecular entanglement and is not easy to be washed off during the spinning process, which will increase the hygroscopicity of the fiber and increase the moisture absorption and swelling ratio of the fiber, causing scratches during the dyeing and finishing of the fabric and affecting the dimensional stability of the fabric. In addition, the boiling point of polyvinyl alcohol (PVC) is relatively high, and the subsequent solvent recovery is not conducive to the seven-effect evaporation recovery. After the addition of polyvinyl alcohol (PVC), it passes through a twin-screw extruder to swell and dissolve to prepare a colloid. A single twin-screw extruder will be limited by its small production capacity, and multiple twin-screw extruders are required, with high equipment costs. Summary of the invention

[0009] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing fiber spinning solution by low-temperature dissolution.

[0010] The present invention provides a method for preparing fiber spinning solution by low-temperature dissolution, comprising the following steps:

[0011] S1) mixing one or more of a low molecular weight alcohol solvent, a low molecular weight ether solvent and a polymer with a high concentration NMMO solution to obtain a mixed solution; the polymer contains one or more of a hydroxyl group, a carboxyl group and an amino group;

[0012] S2) mixing the mixed solution with the crushed pulp to swell, and then heating to 75° C. or above to dissolve, to obtain a fiber spinning solution; the swelling temperature is less than or equal to 55° C.

[0013] Preferably, the mass of one or more of the low molecular weight alcohol solvent, the low molecular weight ether solvent and the polymer is 0.1% to 18% of the mass of the mixed solution.

[0014] Preferably, the mass concentration of the high-concentration NMMO solution is 82% to 87%; the mass concentration of NMMO in the mixed solution is greater than or equal to 72%.

[0015] Preferably, the low molecular weight alcohol solvent is selected from one or more of ethanol, ethylene glycol, glycerol and isopropanol; the low molecular weight ether solvent is selected from one or more of ethyl ether, butyl ether and ethylene glycol diethyl ether; the polymer is selected from one or more of polyvinyl alcohol, polyethylene glycol and dimer alcohol.

[0016] Preferably, the pulverized pulp is granular pulp and / or hand-torn large pulp chunks.

[0017] Preferably, the mass of the crushed pulp is 9% to 19% of the total mass of the crushed pulp and the mixed solution.

[0018] Preferably, the swelling temperature is 50° C. to 55° C.; and the swelling time is 15 to 60 minutes.

[0019] Preferably, the dissolution temperature is 75°C to 98°C; and the dissolution time is 1 to 1.5 hours.

[0020] Preferably, the swelling and dissolving are carried out under stirring conditions; the stirring speed is 60 to 300 rpm.

[0021] Preferably, the dissolution is carried out under vacuum conditions; the vacuum degree of the vacuum conditions is -0.098 MPa.

[0022] The present invention provides a method for preparing fiber spinning solution by low-temperature dissolution, comprising the following steps: S1) mixing a low molecular weight alcohol solvent, a low molecular weight ether solvent and one or more of a polymer with a high concentration NMMO solution to obtain a mixed solution; the polymer contains one or more of a hydroxyl group, a carboxyl group and an amino group; S2) mixing the mixed solution with crushed pulp for swelling, and then heating to 75°C or above for dissolution to obtain a fiber spinning solution; the swelling temperature is less than or equal to 55°C. Compared with the prior art, the present invention performs swelling at a low temperature, is not easy to form an initial dissolution, is conducive to the full penetration and diffusion of the NMMO solution, and the swelling is more complete. At the same time, the added organic matter can increase the penetration of the solution to cellulose, further increasing the swelling effect; further, the added organic matter can be removed by heating or vacuum heating, and the dissolution zone is reached in a short time. The vacuum heating also reduces the dissolution temperature, which saves energy consumption costs while greatly reducing the thermal degradation of cellulose, thereby improving the mechanical properties and strength of cellulose. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] The present invention provides a method for preparing fiber spinning stock solution by low-temperature dissolution, comprising the following steps: S1) mixing one or more of a low molecular weight alcohol solvent, a low molecular weight ether solvent and a polymer with a high concentration NMMO solution to obtain a mixed solution; the polymer contains one or more of a hydroxyl group, a carboxyl group and an amino group; S2) mixing the mixed solution with crushed pulp for swelling, and then heating to 75°C or above for dissolution to obtain a fiber spinning stock solution; the swelling temperature is less than or equal to 55°C.

[0025] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.

[0026] A low molecular weight alcohol solvent, a low molecular weight ether solvent and one or more of the polymers are mixed with a high concentration NMMO solution to obtain a mixed solution; the low molecular weight alcohol solvent can be a low molecular weight alcohol solvent well known to those skilled in the art, without any special restrictions, and preferably one or more of ethanol, ethylene glycol, glycerol and isopropanol in the present invention; the low molecular weight ether solvent can be a low molecular weight ether solvent well known to those skilled in the art, without any special restrictions, and preferably one or more of ethyl ether, butyl ether and ethylene glycol diethyl ether in the present invention; the polymer can be a polymer containing hydroxyl groups well known to those skilled in the art, without any special restrictions, and preferably one or more of polyvinyl alcohol, polyethylene glycol and dimer in the present invention; the molecular weight of the polyvinyl alcohol is preferably 25,000 to 35,000; the molecular weight of the polyethylene glycol is preferably 1000 ~5000, the molecular weight of the dimer alcohol is preferably 537; the mass of one or more of the low molecular weight alcohol solvent, low molecular weight ether solvent and polymer is preferably 0.1% to 18% of the mass of the mixed solution, more preferably 0.1% to 15%, more preferably 0.1% to 10%, more preferably 0.1% to 5%, more preferably 0.1% to 3%, and most preferably 0.1% to 2%; the mass concentration of the high concentration NMMO solution is preferably 82% to 87%, preferably 82.8% to 85%, more preferably 82.8% to 84.5%; the mass concentration of NMMO in the mixed solution is preferably greater than or equal to 72%; when the boiling points of the low molecular weight alcohol solvent, low molecular weight ether solvent and polymer are higher than 110°C, the mass concentration of NMMO in the mixed solution is preferably greater than or equal to 80%, more preferably greater than or equal to 83%.

[0027] The mixed solution is mixed with crushed pulp for swelling; the pulp is preferably hardwood dissolving pulp and / or coniferous wood dissolving pulp (but not limited to), more preferably kraft hardwood dissolving pulp and / or coniferous wood sulfite dissolving pulp; the content of α-cellulose in the pulp is preferably greater than or equal to 90%, more preferably greater than or equal to 95%; the intrinsic viscosity of the pulp is preferably 400-480 ml / g, more preferably 420-460 ml / g, and more preferably 440 ml / g; the Fe content in the pulp is preferably less than 5 ppm; the water content of the pulp is preferably 5%-10%, more preferably 6%-8%, and more preferably 7%; In the present invention, the pulp does not need to be beaten into fluff or too fine particles. It can be completely infiltrated and swollen by adding larger particles or large pulp boards, and a transparent and uniform colloid can be obtained by heating and dissolving. Therefore, in the present invention, the crushed pulp is preferably granular pulp and / or hand-torn large pieces of pulp; the mass of the crushed pulp is preferably 9% to 19% of the total mass of the pulp and the mixed solution, more preferably 10% to 15%, and more preferably 12% to 14%; in the present invention, a stabilizer is preferably added; the type of the stabilizer can be a stabilizer well known to those skilled in the art, and there is no special limitation. In the present invention, it is preferably propyl gallate (PG); the mass of the stabilizer is preferably 0.5% to 10% of the mass of the crushed pulp, more preferably 2% to 8%, more preferably 4% to 6%, and most preferably 4.6%; the swelling temperature is less than or equal to 55°C, preferably 25°C to 55°C; considering the speed and effect of swelling, in the present invention, the swelling temperature is more preferably 50°C to 55°C; the lower temperature makes the medium and high concentration NMMO solution lose its ability to dissolve cellulose or its dissolving ability is greatly weakened, so that the cellulose particles only swell in the high concentration NMMO solution at low temperature, or almost do not dissolve in a short time, and the penetration completely prevents the formation of a gel layer on the surface of the cellulose to prevent further penetration of NMMO; However, the lower the swelling temperature is, the better it is. Although the energy requirement is low at a low temperature, if the temperature is too low, the swelling penetration rate is too slow. Selecting a verified temperature can take into account both energy consumption and swelling rate. Although lowering the temperature reduces the swelling rate, the addition of one or more low molecular weight alcohol solvents, low molecular weight ether solvents and polymers can increase the solution's penetration into cellulose and increase the swelling effect. The swelling is preferably carried out under stirring; the stirring is preferably low-speed stirring; the stirring speed is preferably 60 to 300 rpm; the swelling time is preferably 15 to 60 min, more preferably 20 to 50 min, and even more preferably 30 to 40 min.

[0028] After sufficient swelling, the temperature is raised to 75°C or above for dissolution to obtain a fiber spinning stock solution; the new process of adding a low-boiling point additive changes the evaporation of water into the evaporation of a low-boiling point organic solvent, and a transparent and uniform colloid in good condition can be prepared without vacuuming, which greatly saves energy consumption; the temperature can also be raised to dissolve under vacuum conditions, and low molecular weight organic matter can be quickly evaporated and degassed at the same time, so as to obtain a transparent and uniform colloid in a shorter time; the vacuum degree of the vacuum condition is preferably -0.098MPa; the new process of adding a high-boiling point additive, after sufficient swelling, the temperature is raised to 75°C or above for dissolution, and there is no need to evaporate water to directly obtain a transparent and uniform fiber spinning stock solution; the dissolution temperature is preferably 75°C to 98°C, more preferably 85°C to 98°C, and more preferably 90°C to 95°C; the dissolution time is preferably 1 to 1.5h; the dissolution is preferably carried out under stirring conditions; the stirring is preferably low-speed stirring; the stirring speed is preferably 60 to 300rpm. The swelling and dissolution temperatures are low, which can greatly save energy costs, greatly reduce the thermal degradation of cellulose, significantly improve the mechanical properties and strength of cellulose, and significantly lighten the color of the colloidal solvent, which greatly reduces the burden of anionic and cationic resins for subsequent solvent recovery.

[0029] The present invention performs swelling at low temperature, is not easy to form initial dissolution, is conducive to the full penetration and diffusion of the NMMO solution, and the swelling is more complete. At the same time, the added organic matter can increase the penetration of the solution to the cellulose, further increasing the swelling effect. Furthermore, the added organic matter can be removed by heating or vacuum heating, and reaches the dissolution zone in a short time. The vacuum heating also reduces the dissolution temperature, which saves energy consumption costs while greatly reducing the thermal degradation of cellulose, thereby improving the mechanical property strength of cellulose.

[0030] In order to further illustrate the present invention, a method for preparing fiber spinning solution by low-temperature dissolution provided by the present invention is described in detail below in conjunction with embodiments.

[0031] The reagents used in the following examples are all commercially available; the pulp board model used in the examples is BSC430-Brazilian pulp polymerization degree 430.

[0032] The detection obtained in the embodiment is detected according to the following method:

[0033] 1. Zero shear viscosity of colloid: Use Haake rheometer to measure zero shear viscosity at 85℃;

[0034] 2. Degree of polymerization of colloid: After washing and drying the colloid, grind it into powder, dissolve it in copper ammonia solution and use Ubbelohde viscometer to measure the polymer of fiber in the colloid;

[0035] 3. Chroma of colloid: Add 10g colloid into 500g water, soak it completely, and test the chroma using UV selective absorbance at 400nm.

[0036] Example 1

[0037] Raw materials: 7.471 g of BSC430 large hand-torn pulp board, 0.348 g of propyl gallate (PG), and a mixed solution of 49 g of 84.5% NMMO solution and 1 g of ether.

[0038] The new process direct preparation method is as follows: add 0.348g of PG and 7.471g of hand-torn large pulp board to the mixed solution of 50g NMMO and ether, stir and pre-mix at 500rpm at about 50℃ for about 30min, then heat to 95℃ and react for 1.5h to prepare a uniform and transparent colloid.

[0039] Traditional direct dissolution method: add 0.348g of PG and 7.471g of pulp wool crushed by a grinder to 50g of NMMO heated and melted 84.5% NMMO solution, then heat to 110°C and adjust the speed to about 500rpm, and react for 2.5h to prepare a uniform and transparent colloid.

[0040] The physical and chemical properties of the colloid obtained in Example 1 were tested, and the results are shown in Table 1.

[0041] Table 1 Colloid performance test data of Example 1

[0042] Traditional direct dissolution method New process method Dissolving colloid temperature / ℃ 110 95 Preparation time of colloid / h 2 1 Number of bright spots under the microscope (incompletely dissolved fibers) 1 1 Cellulose content% 13.2 13.2 85℃ Zero shear viscosity 16000 22500 Degree of polymerization of colloid 378 410 Chroma of colloid 725 250

[0043] Example 2

[0044] Raw materials: 7.471 g of BSC430 large hand-torn pulp board, 0.348 g of PG, and a mixed solution of 49.95 g of 82.8% NMMO solution and 0.05 g of polyethylene glycol.

[0045] The new process of direct dissolution preparation method is as follows: PG and hand-torn large pulp boards are added to a mixed solution of 50g NMMO and polyethylene glycol, and the mixture is pre-mixed at about 50°C and 300rpm with stirring for about 30min, and then the temperature is raised to 95°C and reacted for 1.5h to prepare a uniform and transparent colloid.

[0046] Traditional direct dissolution method: add 0.348g of PG and 7.471g of pulp wool crushed by a grinder to 50g of NMMO heated and melted 84.5% NMMO solution, then heat to 110°C and adjust the speed to about 500rpm, and react for 2.5h to prepare a uniform and transparent colloid.

[0047] The physical and chemical properties of the colloid obtained in Example 2 were tested, and the results are shown in Table 1.

[0048] Table 2 Colloid performance test data of Example 2

[0049] Traditional direct dissolution method New process method Dissolving colloid temperature / ℃ 110 95 Preparation time of colloid / h 2 1 Number of bright spots under the microscope (incompletely dissolved fibers) 1 1 Cellulose content% 13.2 13.2 85℃ Zero shear viscosity 16000 22518 Degree of polymerization of colloid 378 411 Chroma of colloid 725 252

[0050] Compared with the traditional method, the new low-temperature swelling method for preparing colloids greatly reduces energy consumption, reduces fiber degradation, increases zero-shear viscosity, and reduces the color of the colloid and the coagulation bath.

Claims

1. A method for preparing fiber spinning solution by low temperature dissolution, characterized in that: The following steps are involved: S1) mixing one or more of a low molecular weight alcohol solvent, a low molecular weight ether solvent and a polymer with a high concentration NMMO solution to obtain a mixed solution; the polymer contains one or more of a hydroxyl group, a carboxyl group and an amino group; S2) mixing the mixed solution with the crushed pulp to swell, and then heating to 75° C. or above to dissolve, to obtain a fiber spinning solution; The mass of one or more of the low molecular weight alcohol solvent, low molecular weight ether solvent and polymer is 0.1% to 18% of the mass of the mixed solution; The mass concentration of the high-concentration NMMO solution is 82% to 87%; the mass concentration of NMMO in the mixed solution is greater than or equal to 72%; The crushed pulp is granular pulp and / or hand-torn large pulp pieces; The mass of the crushed pulp is 9% to 19% of the total mass of the crushed pulp and the mixed solution; The low molecular weight alcohol solvent is selected from one or more of ethanol, ethylene glycol, glycerol and isopropanol; the low molecular weight ether solvent is selected from one or more of ethyl ether, butyl ether and ethylene glycol diethyl ether; the polymer is selected from polyethylene glycol; The swelling temperature is 50°C to 55°C; the swelling time is 15 to 60 minutes; The dissolution temperature is 75°C to 98°C; the dissolution time is 1 to 1.5 hours; The swelling and dissolving are carried out under stirring conditions; the stirring speed is 60 to 300 rpm; The dissolution is carried out under vacuum conditions; the vacuum degree of the vacuum conditions is -0.098MPa.

Citation Information

Patent Citations

  • Method for preparing cellulose spinning fluid

    CN101240461A

  • Method for preparing fiber spinning solution by direct dissolution method

    CN114016141A

  • A solution containing cellulose dissolved in N-methylmorpholine-N-oxide and high tenacity lyocell multifilament using the same

    CN1612958A

  • Production of spinning stock solution

    JP1986275411A

  • Process for the preparation of a cellulose solution for spinning of fibres, filaments or films therefrom

    US20050230860A1