Method for preparing imide-based solid electrolyte, solid electrolyte and related products

By adding side chains that conduct lithium ions to polyimide or forming composite materials, the ionic conductivity is improved, which solves the problem of low conductivity of polyimide solid electrolyte and achieves high mechanical strength and excellent ionic conductivity. Imide-based polymer solid electrolyte enhances the stability and safety performance of lithium metal batteries.

CN115064767BActive Publication Date: 2024-10-22BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210761209.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-29
Publication Date
2024-10-22
Estimated Expiration
2042-06-29

AI Technical Summary

Technical Problem

When polyimide is used as a solid electrolyte, its ionic conductivity is low and cannot meet the needs of lithium metal batteries.

Method used

By adding side chains that conduct lithium ions at the molecular level of polyimide or forming composite materials with other lithium-conducting phases to improve its ionic conductivity, a method for preparing imide-based polymer solid electrolytes is used, including adding diamine The monomer, anhydride monomer and lithium salt are uniformly dispersed in an organic solvent, stirred and heated under vacuum to initiate polymerization to prepare an imide-based polymer solid electrolyte.

Benefits of technology

An imide-based polymer solid electrolyte with high mechanical strength and excellent ionic conductivity has been achieved, which effectively inhibits the growth of lithium dendrites, enhances the stability and safety performance of the battery, and improves the energy density and life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115064767B_ABST
    Figure CN115064767B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method of an imide-based solid electrolyte, a solid electrolyte and related products, and belongs to the field of battery material technology. The steps of the preparation method include: uniformly dispersing a diamine monomer, a dianhydride monomer and a lithium salt in an organic solvent, stirring to obtain a viscous polyamine precursor solution; after the polyamine precursor solution is scraped, vacuum heating is used to induce polymerization of the diamine monomer and the dianhydride monomer to obtain an imide-based polymer solid electrolyte. The present invention selects different monomers, and the monomers have C‑O‑C bonds, S=O bonds, etc., which increases the number of active sites other than ‑C(O)‑N(R)‑C(O)‑, and further improves the ionic conductivity of the solid electrolyte. The ionic conductivity of the imide-based polymer solid electrolyte disclosed in the present invention is 10 ‑5 ‑10 ‑3 S cm ‑1 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a method for preparing an imide-based solid electrolyte, a solid electrolyte and related products. Background Art

[0002] Lithium metal batteries have an ultra-high energy density, with a theoretical specific capacity of 3860mAh g -1 , the lowest redox potential is -3.04 V. However, repeated stripping / embedding of lithium metal batteries in organic liquid electrolytes will produce a large number of lithium dendrites penetrating the diaphragm, leading to internal short circuits and causing a series of safety accidents such as liquid leakage, fire and explosion.

[0003] Solid electrolytes can inhibit the formation of some lithium dendrites due to their good mechanical properties, thereby greatly improving the stability of solid-state lithium metal batteries. Solid electrolytes can be roughly divided into: inorganic solid electrolytes and polymer solid electrolytes. Among them, polymer electrolytes have good ionic conductivity and flexibility, and can form a relatively close interface contact with the electrode, playing a key role in the comprehensive performance of solid-state lithium metal batteries.

[0004] Polymer electrolytes can be divided into ether-based polymer electrolytes, nitrile-based polymer electrolytes, siloxane-based polymer electrolytes, carbonate-based polymer electrolytes, vinylidene fluoride-based polymer electrolytes, polyurethane polymer electrolytes, imide-based polymer electrolytes, etc., according to the type of functional groups. Among them, polyethylene oxide, as a typical ether-based polymer electrolyte, has been widely studied in the past few decades due to its excellent coordination and dissociation properties with lithium salts, interfacial stability with lithium metal, and good mechanical strength. However, polyethylene oxide is still hindered from being widely used in solid-state lithium metal batteries due to its low room temperature ionic conductivity, poor mechanical properties, loose interfacial contact with electrodes, and narrow electrochemical window.

[0005] Polyimide refers to a class of polymers containing an imide ring (-CO-N-CO-) on the main chain. The N in the imide group contains a lone pair of electrons, which is a theoretically possible lithium ion coordination site and can dissolve lithium salts to form polymer-lithium salt complexes. In addition to having polar groups, polyimide has ultra-high mechanical strength and thermal stability while being flexible, and is one of the organic polymer materials with the best comprehensive performance.

[0006] Currently, as an important component of solid-state batteries, solid electrolytes need to meet the following requirements: (1) lithium ion conductivity; (2) electrical insulation to prevent internal short circuits and self-discharge; (3) have a wide electrochemical window to prevent degradation; and (4) high mechanical strength to inhibit the growth of lithium dendrites. Polyimide meets most of the requirements of solid electrolytes, but researchers believe that the lack of flexible side chains and lithium coordination sites in its molecular structure leads to low ionic conductivity and is not suitable for direct use as a solid electrolyte.

[0007] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0008] In order to solve the technical problem of low ion conductivity caused by directly using polyimide as a solid electrolyte in the prior art, a method for preparing an imide-based polymer solid electrolyte, a solid electrolyte and a battery are provided.

[0009] Usually, components that can quickly conduct lithium are added at the molecular level or at the microscopic size. Based on these two strategies, researchers have mainly developed the following two types of polyimide solid electrolytes. (1) Single-phase electrolytes based on polyimide. Side chains that conduct lithium ions are added at the molecular level, for example, rigid polyimide segments and flexible polyethylene oxide segments are copolymerized, or polyethylene oxide side chains are grafted into the polyimide main chain. (2) Composite solid electrolytes based on polyimide. Among them, polyimide is used as a support due to its high mechanical strength and thermal stability, and forms a composite material with other lithium-conducting phases to improve its ionic conductivity.

[0010] Theoretically, the imide group and benzene ring in polyimide are potential lithium binding sites, and the molecular structure is highly modifiable, and its linear structure is very likely to become a fast channel for lithium transport. Therefore, polyimide has a great potential to become a polymer solid electrolyte material that combines high mechanical strength and excellent ionic conductivity.

[0011] In order to achieve the above object, the first aspect of the present invention provides a method for preparing an imide-based polymer solid electrolyte, comprising the steps of:

[0012] The diamine monomer, the dianhydride monomer and the lithium salt are uniformly dispersed in an organic solvent and stirred to obtain a viscous polyamino acid precursor solution;

[0013] After the polyamino acid precursor solution is coated by scraping, vacuum heating is performed to induce polymerization of the diamine monomer and the dianhydride monomer to obtain an imide-based polymer solid electrolyte.

[0014] In some embodiments, the diamine monomer has a functional group coordinated with lithium; preferably, the diamine monomer has an ether bond; more preferably, the diamine monomer is 4,4'-diaminodiphenyl ether.

[0015] In some embodiments, the dianhydride monomer is selected from one or more of pyromellitic dianhydride, 4,4'-oxydiphthalic anhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride.

[0016] In some embodiments, the lithium salt is selected from one or more of lithium perchlorate (LiClO4), lithium nitrate (LiNO3), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium bis(difluorosulfonyl imide) (LiFSI), and lithium bis(trifluoromethylsulfonyl imide) (LiTFSI);

[0017] And / or, the organic solvent is selected from one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), and tetrahydrofuran (THF).

[0018] In some embodiments, the mass ratio of the diamine monomer to the dianhydride monomer is 1:1.01-1.03; preferably, the total mass of the diamine monomer and the dianhydride monomer is 10% of the total mass of the dianhydride monomer, the diamine monomer and the organic solvent; more preferably, the mass of the lithium salt is 20%-50% of the total mass of the diamine monomer and the dianhydride monomer.

[0019] In some embodiments, the stirring time is 10-13 hours.

[0020] In some embodiments, before the vacuum heating, the polyurethane precursor solution is scraped and then left to stand at room temperature for 0.5-1 hour to remove part of the organic solvent. The less organic solvent to be volatilized, the greater the viscosity of the system, the thicker the film thickness after heating and volatilization, and the stronger the mechanical strength of the imide-based polymer solid electrolyte membrane. The content of the organic solvent is controlled so that the imide-based polymer solid electrolyte membrane can be made thin while still ensuring the strength of the membrane.

[0021] In some embodiments, the temperature of the vacuum heating is 60-100° C. and preferably, the heating time is 4-12 hours. The polymerization reaction is initiated by vacuum heating.

[0022] A second aspect of the present invention provides a solid electrolyte prepared by the above-mentioned preparation method.

[0023] A third aspect of the present invention is a battery comprising the imide-based polymer solid electrolyte prepared by the above preparation method or the above solid electrolyte.

[0024] Compared with the prior art, the technical effects achieved by the present invention are as follows:

[0025] (1) N and O (C=O) in the imide bond have lone pairs of electrons, while lithium ions have empty orbitals, which can attract lithium ions and oxygen to form a coordination structure. In the molecular chain, lithium ions and oxygen atoms can continuously undergo a complexation-anti-complexation process to achieve rapid lithium ion migration. In addition, the present invention uses different monomers, which have COC bonds, S=O bonds, etc., to increase the number of active sites and further improve the ionic conductivity of the solid electrolyte. The ionic conductivity of the imide-based polymer solid electrolyte disclosed in the present invention is 10 -5 -10 -3 Scm -1 .

[0026] (2) Since polyimide has a benzene ring and a conjugated effect of an aromatic heterocycle, the main bond energy is large, the intermolecular force is large, and the molecular chain is rigid, the polymer material has excellent mechanical properties. The Young's modulus of the imide-based polymer solid electrolyte disclosed in the present invention can reach 800 MPa. The excellent mechanical strength inhibits the growth of some lithium dendrites and prevents the piercing of "lithium dendrites". It can not only effectively avoid battery short circuits, but also enhance the stability of battery cycles and extend the life of the battery.

[0027] (3) Since polyimide is also self-extinguishing, that is, flame retardant, its safety performance is further improved.

[0028] (4) The present invention can obtain imide-based polymer solid electrolytes with different molecular structures as needed by designing and selecting polyimide monomers. In addition, the obtained imide-based polymer solid electrolyte has the advantages of high room temperature ionic conductivity, high mechanical strength, good thermal stability, optical transparency and adjustable thickness, which makes up for the shortcomings of existing polymer solid electrolytes, such as low ionic conductivity, low mechanical strength and the inability to achieve both ionic conductivity and mechanical strength.

[0029] (5) Since the imide-based polymer solid electrolyte membrane disclosed in the present invention has excellent mechanical properties, the membrane thickness can be less than 20 μm, which can further reduce the internal resistance of the battery after assembly and realize a high energy density battery.

[0030] (6) Polyimide itself has good chemical stability and a high electrochemical window. The solid electrolyte membrane disclosed in the present invention can match high-voltage positive electrodes and strong reducing lithium negative electrodes. Our experimental measurement shows that the oxidation potential of polyimide is 4.6V. Therefore, in theory, it can match positive electrode materials below 4.6V. However, the electrochemical window of polyethylene oxide (PEO), which is the most studied in the prior art, is relatively low at 3.8V. High energy density positive electrodes such as lithium cobalt oxide, layered oxides, and spinel oxides are difficult to match with it and need to be modified.

[0031] (7) The technical solution disclosed in the present invention has good prospects for industrial production. At present, one of the most mature industrial production technologies for preparing polyimide membranes is the casting method. The imide-based polymer solid electrolyte membrane described in the present invention can be well adapted to the industrial polyimide preparation process, which is conducive to mass production and industrial battery assembly. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a photograph of a polyimide solid electrolyte membrane prepared in Example 1 of the present invention;

[0033] Figure 2 is a photograph of the thickness measurement of the polyimide solid electrolyte membrane prepared in Example 1 of the present invention;

[0034] Figure 3 It is a schematic diagram of the test results of electrochemical impedance spectroscopy (a) and Arrhenius curve (b) of a stainless steel-stainless steel symmetrical button cell constructed with a polyimide solid electrolyte prepared in Comparative Example 1 of the present invention;

[0035] Figure 4 This is a schematic diagram of the results of lithium-lithium symmetric battery cycle testing of the polyimide solid electrolyte prepared in Example 1 of the present invention;

[0036] Figure 5 This is a schematic diagram of the monomer polymerization principle of Example 1 of the present invention;

[0037] Figure 6 It is a schematic diagram of the monomer polymerization principle of Example 4 of the present invention. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is described below by specific embodiments in conjunction with the accompanying drawings. It should be understood that one or more steps mentioned in the present invention do not exclude the existence of other methods and steps before and after the combination step, or other methods and steps can be inserted between these explicitly mentioned steps. It should also be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Unless otherwise specified, the numbering of each method step is only for the purpose of identifying each method step, and is not intended to limit the order of arrangement of each method or to define the scope of implementation of the present invention. Changes or adjustments in their relative relationships can also be regarded as the scope of implementation of the present invention without substantial changes in the technical content.

[0039] The sources of the raw materials and instruments used in the examples are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0040] Example 1

[0041] 0.2 g of 4,4'-diaminodiphenyl ether (ODA) after vacuum dehydration treatment was dissolved in a mixed solution of 1.857 ml of NMP and 2.013 ml of DMF, and stirred for 30 minutes to obtain a clear and transparent solution; 0.212 g of LITFSI was added to the above clear solution and stirred for 30 minutes to obtain a first mixed solution; 0.225 g of pyromellitic dianhydride (PMDA) was added to the first mixed solution in small amounts and multiple times to make the reaction more uniform and sufficient, and to prevent the dianhydride monomer from being exposed to the air for a long time to absorb water (the presence of trace water will affect the polymerization), and then a polyamino acid precursor liquid was obtained and stirred at room temperature for 13 hours; an appropriate amount of the precursor liquid was scraped onto a clean glass substrate using a 300 μm scraper, and the organic solvent was volatilized at room temperature for 1 hour, and then vacuum dried at 80°C for 4 hours to obtain the following: Figure 1 The PMDA-ODA polyimide solid electrolyte membrane shown.

[0042] Example 2

[0043] 0.2 g of 4,4'-diaminodiphenyl ether (ODA) after vacuum dehydration treatment was dissolved in a mixed solution of 2.486 ml of NMP and 2.695 ml of DMF, and stirred for 30 minutes to obtain a clear and transparent solution; 0.285 g of LITFSI was added to the above clear solution and stirred for 30 minutes to obtain a first mixed solution; 0.369 g of 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride was added to the first mixed solution in small amounts and multiple times to obtain a polyamino acid precursor liquid and stirred at room temperature for 13 hours; an appropriate amount of the precursor liquid was scraped onto a clean glass substrate using a 300 μm scraper, the organic solvent was volatilized at room temperature for 1 hour, and then vacuum dried at 80°C for 4 hours.

[0044] Example 3

[0045] 0.2 g of 4,4'-diaminodiphenyl ether (ODA) after vacuum dehydration treatment was dissolved in a mixed solution of 2.272 ml of NMP and 2.463 ml of DMF, and stirred for 30 minutes to obtain a clear and transparent solution; 0.285 g of LITFSI was added to the above clear solution and stirred for 30 minutes to obtain a first mixed solution; 0.320 g of 4,4'-oxydiphthalic anhydride (ODPA) was added to the first mixed solution in small amounts and multiple times to obtain a polyamino acid precursor liquid and stirred at room temperature for 13 hours; an appropriate amount of the precursor liquid was scraped onto a clean glass substrate using a 300 μm scraper, the organic solvent was volatilized at room temperature for 1 hour, and then vacuum dried at 80°C for 4 hours.

[0046] Example 4

[0047] 0.2 g of 4,4'-diaminodiphenyl ether (ODA) after vacuum dehydration treatment was dissolved in a mixed solution of 1.992 ml of NMP and 2.094 ml of DMF, and stirred for 30 minutes to obtain a clear and transparent solution; 0.228 g of LITFSI was added to the above clear solution and stirred for 30 minutes to obtain a first mixed solution; 0.256 g of bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (DMBD) was added to the first mixed solution in small amounts and multiple times to obtain a polyamino acid precursor liquid and stirred at room temperature for 13 hours; an appropriate amount of the precursor liquid was scraped onto a clean glass substrate using a 300 μm scraper, the organic solvent was volatilized at room temperature for 1 hour, and then vacuum dried at 80°C for 4 hours.

[0048] test

[0049] Thickness measurement:

[0050] like Figure 2 As shown, the thickness of the film prepared in Example 1 was measured and found to be 13 μm.

[0051] Ionic conductivity test:

[0052] The ionic conductivity of the imide-based polymer solid electrolyte prepared in Example 1 was tested by the AC impedance method. The solid electrolyte was equipped in a stainless steel||stainless steel symmetrical button cell, and the AC impedance spectrum of the electrolyte was measured using an electrochemical workstation (frequency range: 1000KHz-1Hz), and the ionic conductivity was calculated according to the formula σ=L / (R×S). Wherein, σ is the ionic conductivity of the electrolyte, L is the thickness of the electrolyte, R is the resistance value of the electrolyte, and S is the contact area between the electrolyte and the test electrode. Figure 3(a) and (b) are the impedance spectra and Arrhenius curves of the PMDA-ODA polyimide solid electrolyte prepared in Example 1 at different temperatures. The room temperature ionic conductivity of the PMDA-ODA polyimide solid electrolyte is calculated to be 1.44*10 -5 S cm -1 , the ionic conductivity is 1.82*10 at 80℃ -4 S cm -1 In addition, the change of ionic conductivity of the solid electrolyte with temperature was also studied. As the temperature increases, the ionic conductivity of the PMDA-ODA polyimide solid electrolyte prepared in Example 1 significantly increases. This is mainly due to the rapid migration of lithium ions at high temperatures, which is conducive to improving the ionic conductivity of PMDA-ODA.

[0053] Ion migration number test:

[0054] The Li||Li symmetrical battery equipped with the solid electrolyte prepared in Example 1 was measured using an electrochemical workstation to measure the AC impedance spectrum of the battery to obtain the resistance value before DC polarization. The current-time curve of the electrolyte was then measured for 5000s and a bias voltage of 10mV. Then, the AC impedance spectrum after DC polarization was measured to obtain the resistance value after DC polarization. According to the formula t=I s (ΔV-I0R0) / I0(ΔV-I s R s ) is used to calculate the migration number of the electrolyte. Where t is the migration number of the electrolyte, ΔV is the bias voltage, I0 is the initial current value, R0 is the initial resistance value, I s is the steady-state current value after DC polarization, R s is the resistance value after DC polarization. The ion migration number of the PMDA-ODA polyimide solid electrolyte prepared in Example 1 is calculated to be 0.38.

[0055] Electrochemical stability test:

[0056] The solid electrolyte prepared in Example 1 was subjected to an electrochemical stability test. A Li||steel sheet battery equipped with a solid electrolyte was used to measure a linear sweep voltammetry (LSV) curve (voltage range: open circuit voltage -5 V, scan rate: 1 mV / s). The oxidation stability of the solid electrolyte reached 4.6 V.

[0057] Cyclic voltammetry curve test:

[0058] The solid electrolyte prepared in Example 1 was subjected to a lithium-lithium symmetric battery cycle test. At 30°C, the current density was 0.1 mA cm -2 The battery cycle was 550 hours with no significant increase in voltage polarization. Figure 4As shown, the cycle is stable within 550 hours.

[0059] The above properties of the imide-based solid electrolytes prepared in Examples 2-4 were tested, and all obtained 10 -5 -10 -3 Scm -1 The room temperature ionic conductivity, the ion migration number above 0.3, and the room temperature lithium-lithium symmetric battery cycle test are excellent, which are consistent with Example 1.

[0060] Figure 5 is the reaction mechanism of Example 1, Figure 6 The reaction mechanism of Example 3 is shown in Figure 3. They all have the performance of conducting lithium ions, and the difference is mainly reflected in the level of ionic conductivity. Compared with PMDA and ODPA, PMDA has a benzene ring, and ODPA has two benzene rings connected by an ether bond. In addition to the N and C=O in the imide bond having lone pairs of electrons that can attract lithium ions as active sites, since the ether oxygen has lone pairs of electrons and the lithium ions have empty orbitals, they can form a coordination structure with oxygen. The lithium ions and oxygen atoms in the chain segments can continuously undergo a complexation-anti-complexation process, and the migration of lithium ions can be achieved by intra-chain / inter-chain hopping in the polymer electrolyte, thereby further improving the ionic conductivity. Secondly, the mechanical properties of the membrane are also different. ODPA is more flexible than PMDA molecular chains (two benzene rings are connected by a single bond), so the flexibility of the membrane is better. The other different embodiments are also based on the same principle. By screening different polyimide monomers, imide-based polymer solid electrolytes with different molecular structures are prepared.

[0061] Example 5

[0062] A lithium metal battery comprises a positive electrode, a negative electrode and the PMDA-ODA polyimide solid electrolyte prepared in Example 1.

[0063] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing an imide-based polymer solid electrolyte, characterized in that: The steps of the preparation method include: The diamine monomer, the dianhydride monomer and the lithium salt are uniformly dispersed in an organic solvent, and stirred to obtain a viscous polyamino acid precursor solution; specifically, the diamine monomer is first dissolved in an organic solvent, and then the lithium salt is dissolved in the organic solution of the diamine monomer, and then the dianhydride monomer is added, and stirred to obtain a viscous polyamino acid precursor solution; After the polyamino acid precursor solution is coated by a scraper, vacuum heating is performed to initiate polymerization of the diamine monomer and the dianhydride monomer to obtain an imide-based polymer solid electrolyte; The diamine monomer is 4,4'-diaminodiphenyl ether; The mass ratio of the diamine monomer to the dianhydride monomer is 1:1.01-1.03; The total mass of the diamine monomer and the dianhydride monomer is 10% of the total mass of the dianhydride monomer, the diamine monomer and the organic solvent; The mass of the lithium salt is 20%-50% of the total mass of the diamine monomer and the dianhydride monomer.

2. The preparation method according to claim 1, characterized in that: The dianhydride monomer is selected from one or more of pyromellitic dianhydride, 4,4'-oxydiphthalic anhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride.

3. The preparation method according to claim 1, characterized in that: The lithium salt is selected from one or more of lithium perchlorate, lithium nitrate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluorosulfonylimide), and lithium bis(trifluoromethylsulfonylimide).

4. The preparation method according to claim 1, characterized in that: The organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide and tetrahydrofuran.

5. The preparation method according to claim 1, characterized in that: The stirring time is 10-13h.

6. The preparation method according to claim 1, characterized in that: Before the vacuum heating, the polyurethane precursor solution is scraped and then allowed to stand at room temperature for 0.5-1 hour to remove part of the organic solvent.

7. The preparation method according to claim 1, characterized in that: The temperature of the vacuum heating is 60-100°C.

8. The preparation method according to claim 1, characterized in that: The vacuum heating time is 4-12h.

9. A solid electrolyte prepared according to the preparation method according to any one of claims 1 to 8.

10. A battery, characterized in that: It comprises the imide-based polymer solid electrolyte prepared by the preparation method according to any one of claims 1 to 8 or the solid electrolyte according to claim 9.