A carbon-supported niobium pentoxide microsphere and its preparation method and application

By using the carbon-supported niobium pentoxide microsphere structure in lithium-ion batteries, the problem of insufficient electrochemical performance of the negative electrode material of lithium-ion batteries is solved, high power density and safety are achieved, and it is suitable for fast-charging lithium-ion batteries.

CN115133017BActive Publication Date: 2024-10-29WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210829530.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-10-29
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials have insufficient electrochemical performance under fast discharge/charge and high-rate conditions, making it difficult to achieve high power density and safety requirements. In particular, niobium pentoxide, as an electronic insulator, results in low conductivity, which limits lithium High power density of ion batteries.

Method used

Using carbon-supported niobium pentoxide microspheres, a uniform and dense spherical structure formed by dense accumulation of niobium pentoxide nanoparticles and carbon networks, prepared by hydrothermal method and post-heat treatment, combined with conductive agents and adhesives for lithium Ion battery anode material to improve electronic conductivity and cycle stability.

Benefits of technology

It achieves high volume capacity and mass load, improves the specific capacity and rate performance of lithium-ion batteries, significantly improves electrochemical performance, is suitable for fast-charging lithium-ion batteries, and has excellent cycle stability and high safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003745232040000011
    Figure HDA0003745232040000011
  • Figure HDA0003745232040000012
    Figure HDA0003745232040000012
  • Figure HDA0003745232040000013
    Figure HDA0003745232040000013
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrochemical energy materials, and discloses a carbon-supported niobium pentoxide microsphere and its preparation method and application. The preparation method comprises mixing a niobium source, a surfactant, an organic ligand and ethanol evenly to obtain a precursor solution; heating the precursor solution for hydrothermal reaction to obtain a precursor; and sintering the precursor at high temperature to obtain carbon-supported niobium pentoxide microspheres. The carbon-supported niobium pentoxide microsphere prepared by the present invention has a particle size of 1-2 μm, is formed by densely stacking niobium pentoxide nanoparticles and a carbon network, has excellent electrochemical properties, and can be widely used in the field of electrochemical energy storage; when used as a negative electrode active material of a lithium ion battery, it exhibits a high specific capacity, good cycle stability and excellent rate performance, and is a potential application material for fast-charging lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical energy materials, and specifically relates to a carbon-supported niobium pentoxide microsphere and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have been commercialized in recent years due to their high energy density. With the development of smart electronic products and electric vehicles, the development of lithium-ion batteries with high power density has become one of the main challenges. However, for commercial graphite-based anode materials, they have slow lithium ion diffusion kinetics, making it difficult to achieve fast discharge / charge, and therefore cannot meet the requirements of high power density. In addition, when the operating voltage is low, it is easy to cause safety problems such as short circuits, which is particularly serious at high rates. Although other insertion materials such as Li4Ti5O 12 (LTO) has excellent rate performance and safe working potential (1.55V vs Li + / Li), but the low theoretical capacity limits its energy density. Therefore, there is an urgent need to develop negative electrode materials with high rate, high safety and high energy density.

[0003] Recently, orthorhombic niobium pentoxide (T-Nb2O5) has been widely studied in lithium-ion batteries due to its small volume change, high capacity, high rate behavior and safe working potential (1.1-2V). In the structure of T-Nb2O5, there are many octahedral voids between its (001) planes, which provide fast ion transport tunnels and thus have high ionic conductivity. However, T-Nb2O5 is an electronic insulator with low electrical conductivity, which greatly limits the high power density of lithium-ion batteries. To solve this problem, various strategies must be developed to improve it and enhance its electrochemical performance. Among them, combining various carbon materials with Nb2O5 is an effective method to improve electronic conductivity. In addition, nanostructured Nb2O5, such as nanoparticles, nanosheets, nanowires, etc., can be designed to have a smaller ion and electron diffusion distance during the charge / discharge process. However, Nb2O5 nanostructures with low tap density are difficult to be used in commercial electrodes with high loading. At the same time, the high specific surface area increases the reaction interface between the electrode and the electrolyte, resulting in side reactions and poor long-cycle performance. Compared with nanostructured Nb2O5, micron-sized Nb2O5 with higher tap density is more likely to meet the needs of actual batteries. At the same time, in order to achieve high area capacity and excellent cycle performance under high load conditions, micron-sized Nb2O5 is required to have higher ionic and electronic conductivity over a longer diffusion distance. Therefore, further exploration and preparation of carbon-supported Nb2O5 microstructures are of great significance for improving the electrochemical properties of Nb2O5 and accelerating its promotion and application in batteries. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a carbon-supported niobium pentoxide microsphere and a preparation method and application thereof in view of the deficiencies of existing materials in terms of electrochemical performance. The microsphere is formed by dense accumulation of niobium pentoxide nanoparticles and a carbon network, presenting a uniform and dense solid sphere structure, having excellent electrochemical properties, and can be widely used in the field of electrochemical energy storage, especially in the field of negative electrode materials for lithium-ion batteries.

[0005] In order to solve the technical problem proposed by the present invention, the present invention provides a method for preparing carbon-supported niobium pentoxide microspheres, comprising the following steps:

[0006] 1) dissolving a niobium source and a surfactant in ethanol to form a mixed solution A;

[0007] 2) dissolving the organic ligand in ethanol to form a mixed solution B;

[0008] 3) Mixing the mixed solution A and the mixed solution B uniformly to prepare a precursor solution;

[0009] 4) heating the precursor solution to perform a hydrothermal reaction, performing solid-liquid separation after the reaction, washing and drying the obtained solid to obtain a precursor;

[0010] 5) Sintering the precursor at high temperature to obtain carbon-supported niobium pentoxide microspheres.

[0011] In the above scheme, the niobium source is niobium pentachloride.

[0012] In the above scheme, the surfactant is polyvinyl pyrrolidone.

[0013] In the above scheme, the organic ligand is dimethylimidazole.

[0014] In the above scheme, the mass ratio of the niobium source to the surfactant is (1-2):1.

[0015] In the above scheme, the molar ratio of the organic ligand to the niobium source is (10-15):1.

[0016] In the above scheme, step 1) is carried out under the protection of an inert atmosphere to avoid oxidation of the niobium source.

[0017] In the above scheme, in step 1), the volume ratio of the amount of the niobium source substance to ethanol is 1 mmol: (15-23) mL.

[0018] In the above scheme, in step 2), the volume ratio of the amount of the organic ligand to ethanol is 1 mmol: (1-1.6) mL.

[0019] In the above scheme, in step 4), the hydrothermal temperature is 160-220° C., and the hydrothermal time is 6-24 h.

[0020] In the above scheme, in step 4), the washing process is to wash with ethanol 3-6 times.

[0021] In the above scheme, in step 4), the drying temperature is 60-70° C. and the drying time is 12-24 hours.

[0022] In the above scheme, in step 5), the sintering process is to heat the temperature to 750-850°C at a heating rate of 2-5°C / min under the protection of an inert atmosphere, keep the temperature for 3-6 hours, and then cool to room temperature.

[0023] The present invention also provides a carbon-supported niobium pentoxide micron sphere, which is prepared according to the above preparation method. The carbon-supported niobium pentoxide micron sphere has a particle size of 1-2 μm and is formed by densely stacking niobium pentoxide nanoparticles and an internally connected carbon network.

[0024] The present invention also provides an application of carbon-supported niobium pentoxide microspheres in lithium-ion batteries, and the application method is as follows: the carbon-supported niobium pentoxide microspheres are used as negative electrode active materials, added into a solvent together with a conductive agent and an adhesive, mixed evenly, coated on a copper foil, and dried to obtain a negative electrode sheet of a lithium-ion battery; the negative electrode sheet of a lithium-ion battery is used to assemble a lithium-ion battery.

[0025] In the above solution, the conductive agent is acetylene black.

[0026] In the above solution, the adhesive is polyvinylidene fluoride.

[0027] In the above scheme, the solvent is N-methylpyrrolidone.

[0028] In the above solution, the mass ratio of the negative electrode active material, the conductive agent and the adhesive is 7:2:1.

[0029] In the above scheme, the mass volume ratio of the adhesive to the solvent is 10 mg:1 mL.

[0030] In the above scheme, the drying temperature is 60-80°C.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1) In the preparation process of the present invention, a mismatch reaction occurs during the hydrothermal process due to the mismatch of the bond angle between pentavalent niobium ions and dimethylimidazole. Polyvinyl pyrrolidone is used as a surfactant to reduce the rate of the mismatch reaction, so that a uniform micron sphere precursor is formed during the reaction process. The precursor is then subjected to in-situ pyrolysis, and the morphology of the precursor is well maintained. The carbon-supported niobium pentoxide micron spheres finally obtained have a uniform and dense morphology, a particle size of 1-2 μm, a uniform distribution of internal components, and no disordered agglomeration phenomenon occurs, which can effectively promote the electrochemical performance of the micron spheres.

[0033] 2) The microspheres prepared by the present invention are densely stacked with niobium pentoxide nanoparticles and an internally connected carbon network. Compared with nanoscale materials, they have a higher tap density and can achieve high volume capacity and high mass load. At the same time, carbon can provide an electron transmission path to further improve the overall electronic conductivity of the material. The material can be widely used in the field of electrochemical energy storage. When used as a negative electrode active material for lithium-ion batteries, it exhibits a high specific capacity, good cycle stability, and excellent rate performance. Under high load conditions, it can also exhibit high capacity and excellent cycle stability, and is a potential application material for fast-charge lithium-ion batteries.

[0034] 3) The present invention adopts a simple hydrothermal method combined with a later heat treatment, has a simple preparation process, mild conditions, can achieve controllable synthesis of products, meets the requirements of green chemistry, and is conducive to market promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 a) XRD pattern, b) SEM pattern, c) TEM pattern, and dh) EDS mapping pattern of the precursor prepared in Example 1;

[0036] Figure 2 a) XRD graph, b) SEM graph, c) TEM graph, and dh) EDS mapping graph of the carbon-supported niobium pentoxide microspheres prepared in Example 1;

[0037] Figure 3 a) STEM image, b) TEM image, c) ADF image, and df) EDS mapping image of the cross section of the carbon-supported niobium pentoxide microsphere prepared in Example 1;

[0038] Figure 4 a) Raman graph, b) TG graph, and c) BET graph of the carbon-supported niobium pentoxide microspheres prepared in Example 1;

[0039] Figure 5 The lithium ion half-battery prepared in Example 1 is a) at 0.1A·g -1Cycle diagram under current density, b) rate performance diagram under different current density, c) at 2A·g -1 Long cycle diagram under current density;

[0040] Figure 6 The figures are: a) a cycle comparison diagram under different load amounts and b) a relationship diagram between surface capacity and surface load amount of the lithium-ion half-battery prepared in Application Example 1. DETAILED DESCRIPTION

[0041] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0042] Example 1

[0043] A method for preparing carbon-supported niobium pentoxide microspheres comprises the following steps:

[0044] 1) Weigh 0.27 g of niobium pentachloride and 0.25 g of polyvinyl pyrrolidone, and dissolve them in 18 mL of ethanol under an argon atmosphere to form a colorless and transparent mixed solution A;

[0045] 2) Weigh 0.9 g of dimethylimidazole and dissolve it in 17 mL of ethanol to form a colorless and transparent mixed solution B;

[0046] 3) Mixing the mixed solution A and the mixed solution B uniformly to obtain a colorless and transparent precursor solution;

[0047] 4) placing the precursor solution in a reaction kettle, heating it to 200°C for hydrothermal reaction, performing solid-liquid separation after reacting for 12 hours, washing the obtained solid with ethanol three times, and drying it in an oven at 70°C for 12 hours to obtain a precursor;

[0048] 5) placing the precursor in a high temperature tube furnace, heating the temperature to 750° C. at a heating rate of 2° C. / min under the protection of an argon atmosphere, keeping the temperature for 3 hours, and then cooling to room temperature to obtain carbon-supported niobium pentoxide microspheres.

[0049] Figure 1 a) XRD pattern, b) SEM pattern, c) TEM pattern, and dh) EDS mapping pattern of the precursor prepared in this example; the XRD pattern shows that the precursor has no obvious diffraction peak and is amorphous; the EDS mapping pattern shows that the element distribution is Nb, O, N, and C; the SEM and TEM patterns show that the precursor is a uniform solid microsphere with a spherical size of 1-2 μm and a uniform morphology and size.

[0050] Figure 2a) XRD, b) SEM, c) TEM and d) EDS mapping of the carbon-supported niobium pentoxide microspheres prepared in this embodiment; the XRD graph shows that the phase of the carbon-supported niobium pentoxide microspheres is Nb2O5, and the diffraction peak corresponds to the orthorhombic Nb2O5 standard card, without other impurity phases; the EDS mapping graph shows that the element distribution is Nb, O, N and C; the SEM and TEM graphs show that the carbon-supported niobium pentoxide microspheres are uniform solid microspheres with a spherical size of 1-2 μm and a uniform morphology and size, which is consistent with the morphology of the precursor.

[0051] The carbon-supported niobium pentoxide microspheres prepared in this embodiment were cut and polished using a focused ion beam to obtain a cross section. Figure 3 a) STEM image, b) TEM image, c) ADF image, and d) EDS mapping image of the cross section of the carbon-supported niobium pentoxide microsphere prepared in this embodiment; the STEM, TEM and ADF images show that the cross section is composed of multiple Nb2O5 nanoparticles, and carbon is embedded in the single crystal Nb2O5 nanoparticles; the EDS mapping image shows that Nb and C are unevenly distributed in the entire cross section, Nb is distributed in the bright contrast area, C is distributed in the entire cross section area, and the dark contrast area is filled with carbon.

[0052] Figure 4 a) Raman graph, b) TG graph, and c) BET graph of the carbon-supported niobium pentoxide microspheres prepared in this example; the BET graph shows that the specific surface area of ​​the microspheres is 6.67 m 2 g -1 , confirming that carbon-supported niobium pentoxide microspheres have a higher tap density; the TG graph shows that the carbon content of the microspheres is about 5%, which improves the conductivity while ensuring its higher specific capacity; the Raman graph shows that the carbon has a higher degree of graphitization, which improves the overall electronic conductivity of the material.

[0053] Application Example 1

[0054] Application of carbon-supported niobium pentoxide microspheres in lithium-ion batteries, and the application method is as follows:

[0055] Weigh 70 mg of the carbon-supported niobium pentoxide microspheres prepared in Example 1 as the negative electrode active material, 20 mg of acetylene black as the conductive agent, and 10 mg of polyvinylidene fluoride as the binder, add them together in 1 mL of N-methylpyrrolidone and mix them evenly, apply them on copper foil, and dry them at 70°C to obtain a negative electrode sheet for a lithium ion battery; cut the negative electrode sheet for a lithium electronic battery into pieces with an area of ​​0.78 cm 2 The total weight of the disc is 1.5 mg, and the area mass loading is 1.92 mg cm -2, assembled with lithium metal electrode sheets into a lithium-ion half-cell.

[0056] Figure 5 The lithium ion half-battery prepared in this application example has a) at 0.1A·g -1 Cyclic diagram under current density, b) rate performance diagram under different current density, c) at 2A·g -1 Long cycle diagram under current density; Figure a shows that the lithium-ion half-cell is -1 At the current density, it still has a high capacity of 196 mAh g after 100 cycles. -1 The discharge capacity of the lithium-ion half-cell is shown in Figure b. The current density can be increased from 0.1A·g -1 Gradually increase to 6A·g -1 , at 6A·g -1 At high current density, its specific capacity can reach 124 mAh g -1 , and the current density returns to 0.1A·g -1 Its specific capacity can reach 215 mAh g -1 ; Figure c shows that at 2A·g -1 After 2000 cycles, the specific capacity can reach 106 mAh g -1 , demonstrating very excellent cycle stability.

[0057] Figure 6 Figure 1 shows a) a cycle comparison diagram of the lithium-ion half-battery prepared in this application example at different loading levels and b) a relationship diagram between surface capacity and surface loading level. Figure 1 shows that the surface capacity of the lithium-ion half-battery prepared in this application example is 1.5, 3.8, 7.6, and 12.8 mg·cm -2 Under the condition of loading amount, the specific capacity can reach 202.7, 188.8, 186.5, and 171.5 mAh g -1 , showing a high capacity; Figure b shows that at 12.8 mg cm -2 2.05 mAh cm under high load conditions -2 The surface capacity of carbon-supported niobium pentoxide microspheres was confirmed to have excellent electrochemical performance.

[0058] Example 2

[0059] A method for preparing carbon-supported niobium pentoxide microspheres comprises the following steps:

[0060] 1) Weigh 0.54 g of niobium pentachloride and 0.4 g of polyvinyl pyrrolidone, and dissolve them in 45 mL of ethanol under an argon atmosphere to form a colorless and transparent mixed solution A;

[0061] 2) Weigh 1.74 g of dimethylimidazole and dissolve it in 25 mL of ethanol to form a colorless and transparent mixed solution B;

[0062] 3) Mixing the mixed solution A and the mixed solution B uniformly to obtain a colorless and transparent precursor solution;

[0063] 4) placing the precursor solution in a reaction kettle, heating it to 200° C. for hydrothermal reaction, performing solid-liquid separation after reacting for 12 hours, washing the obtained solid with ethanol 4 times, and drying it in an oven at 70° C. for 16 hours to obtain a precursor;

[0064] 5) placing the precursor in a high temperature tube furnace, under the protection of an argon atmosphere, heating the temperature to 800° C. at a heating rate of 3° C. / min, keeping the temperature for 4 hours, and then cooling to room temperature to obtain carbon-supported niobium pentoxide microspheres.

[0065] Example 3

[0066] A method for preparing carbon-supported niobium pentoxide microspheres comprises the following steps:

[0067] 1) Weigh 0.27 g of niobium pentachloride and 0.18 g of polyvinyl pyrrolidone, and dissolve them in 20 mL of ethanol under an argon atmosphere to form a colorless and transparent mixed solution A;

[0068] 2) Weigh 1.2 g of dimethylimidazole and dissolve it in 15 mL of ethanol to form a colorless and transparent mixed solution B;

[0069] 3) Mixing the mixed solution A and the mixed solution B uniformly to obtain a colorless and transparent precursor solution;

[0070] 4) placing the precursor solution in a reaction kettle, heating it to 200°C for hydrothermal reaction, performing solid-liquid separation after reacting for 24 hours, washing the obtained solid with ethanol for 5 times, and drying it in an oven at 70°C for 18 hours to obtain a precursor;

[0071] 5) placing the precursor in a high temperature tube furnace, under the protection of an argon atmosphere, heating the temperature to 800° C. at a heating rate of 4° C. / min, keeping the temperature for 5 hours, and then cooling to room temperature to obtain carbon-supported niobium pentoxide microspheres.

[0072] Example 4

[0073] A method for preparing carbon-supported niobium pentoxide microspheres comprises the following steps:

[0074] 1) Weigh 0.27 g of niobium pentachloride and 0.15 g of polyvinyl pyrrolidone, and dissolve them in 20 mL of ethanol under an argon atmosphere to form a colorless and transparent mixed solution A;

[0075] 2) Weigh 1 g of dimethylimidazole and dissolve it in 15 mL of ethanol to form a colorless and transparent mixed solution B;

[0076] 3) Mixing the mixed solution A and the mixed solution B uniformly to obtain a colorless and transparent precursor solution;

[0077] 4) placing the precursor solution in a reaction kettle, heating it to 180°C for hydrothermal reaction, performing solid-liquid separation after reacting for 24 hours, washing the obtained solid with ethanol for 6 times, and drying it in an oven at 70°C for 24 hours to obtain a precursor;

[0078] 5) placing the precursor in a high temperature tube furnace, under the protection of an argon atmosphere, heating the temperature to 850° C. at a heating rate of 5° C. / min, keeping the temperature for 6 hours, and then cooling to room temperature to obtain carbon-supported niobium pentoxide microspheres.

[0079] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A method for preparing carbon-supported niobium pentoxide microspheres, characterized in that: The following steps are involved: 1) dissolving a niobium source and a surfactant in ethanol to form a mixed solution A; wherein the niobium source is niobium pentachloride, the surfactant is polyvinyl pyrrolidone, and the mass ratio of the niobium source to the surfactant is (1-2):1; 2) dissolving an organic ligand in ethanol to form a mixed solution B; wherein the organic ligand is dimethylimidazole, and the molar ratio of the organic ligand to the niobium source is (10-15):1; 3) Mixing the mixed solution A and the mixed solution B uniformly to prepare a precursor solution; 4) heating the precursor liquid for hydrothermal reaction at a hydrothermal temperature of 160-220° C. for a hydrothermal time of 6-24 h, performing solid-liquid separation after the reaction, washing and drying the obtained solid to obtain a precursor; 5) The precursor is subjected to high temperature sintering to obtain carbon-supported niobium pentoxide microspheres, which are densely stacked niobium pentoxide nanoparticles and a carbon network, and the particle size is 1-2 μm.

2. The method for preparing carbon-supported niobium pentoxide microspheres according to claim 1, characterized in that: In step 1), the volume ratio of the amount of the niobium source to ethanol is 1 mmol: (15-23) mL.

3. The method for preparing carbon-supported niobium pentoxide microspheres according to claim 1, characterized in that: In step 2), the volume ratio of the amount of the organic ligand to ethanol is 1 mmol: (1-1.6) mL.

4. The method for preparing carbon-supported niobium pentoxide microspheres according to claim 1, characterized in that: In step 4), the drying temperature is 60-70° C. and the drying time is 12-24 hours.

5. The method for preparing carbon-supported niobium pentoxide microspheres according to claim 1, characterized in that: In step 4), the washing process is washing with ethanol 3-6 times.

6. The method for preparing carbon-supported niobium pentoxide microspheres according to claim 1, characterized in that: In step 5), the sintering process is to heat the material to 750-850°C at a heating rate of 2-5°C / min under the protection of an inert atmosphere, keep the temperature for 3-6 hours, and then cool the material to room temperature.

7. A carbon-supported niobium pentoxide microsphere prepared by the method according to any one of claims 1 to 6, characterized in that: The carbon-supported niobium pentoxide microsphere has a particle size of 1-2 μm and is formed by stacking niobium pentoxide nanoparticles and an internally connected carbon network.

8. Use of the carbon-supported niobium pentoxide microspheres as claimed in claim 7 in lithium-ion batteries.

Citation Information

Patent Citations

  • Preparation method of carbon composite niobium pentoxide material with micro-nano structure for lithium-ion battery

    CN106252592A

  • Niobium pentoxide / carbon double-quantum-dot nanometer composite material, method for preparing same and application of niobium pentoxide / carbon double-quantum-dot nanometer composite material

    CN108448104A