A method for detecting storage stability of SBS modified asphalt

Through fluorescence microscopy and image processing technology, a data model of phase content and isolation relationship was established, which solved the accuracy and efficiency of polymer modified asphalt stability detection in the prior art, and achieved rapid and accurate modified asphalt stability Testing, suitable for a variety of modifiers and matrix bitumen.

CN115165834BActive Publication Date: 2024-12-03HAIYUN (HAINAN) MATERIALS TECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210932043.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-04
Publication Date
2024-12-03
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

The existing detection methods have low accuracy when evaluating the storage stability of polymer modified asphalt and have a long detection period, so it is impossible to accurately quantify the impact of different modifier content and matrix asphalt phase on stability, resulting in large errors.

Method used

Fluorescent samples were prepared by fluorescence microscope, heated and cooled by hot drop slide method, and obtained fluorescence samples. Combined with picture processing software to calculate phase content, establish a data model of phase content and isolation relationship, and achieve rapid stability of SBS modified asphalt , accurate detection.

Benefits of technology

By quantitatively analyzing the phase state and establishing a model, the accuracy and efficiency of detection are improved, and the detection time is reduced. It is suitable for the phase state of different modifier content and matrix asphalt, and the quality control of modified asphalt is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115165834B_ABST
    Figure CN115165834B_ABST
Patent Text Reader

Abstract

The present invention provides a method for detecting the storage stability of SBS modified asphalt, comprising the following steps: a) preparing a fluorescent sample using SBS modified asphalt, and detecting the phase content of the SBS modified asphalt; b) substituting the phase content of the SBS modified asphalt obtained in step a) into a data model of the relationship between phase content and segregation, obtaining segregation data, and completing the detection of the storage stability of the SBS modified asphalt; the data model of the relationship between phase content and segregation is: #imgabs0# wherein x is the phase content, and y is the segregation index. Compared with the prior art, the detection method provided by the present invention can quantitatively analyze the phase states of different modifier contents and different matrix asphalt phase states and establish a model between segregation, so that the detection of modified asphalt segregation is more accurate, efficient, and convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road material detection, and more specifically to a method for detecting the storage stability of SBS modified asphalt. Background Art

[0002] The stability of polymer modified asphalt directly affects the performance of modified asphalt. If modified asphalt segregates, the modified asphalt will be unusable, causing great economic losses. The current method for testing stability is to test the segregation of modified asphalt. After heating the asphalt sample, pour it into the segregation tube, seal it after cooling, place it vertically in a 163℃ oven for 48±1h, then take it out and place it in a refrigerator for 4h. After freezing, take it out of the refrigerator, divide the asphalt in the segregation test tube into three parts: upper, middle and lower. Detect the softening point of the upper and lower parts of the segregation tube, and calculate the difference between the softening points of the upper and lower parts. The difference between the softening points of the upper and lower parts is required to be no more than 2.5℃ for the segregation to be qualified. However, the total time for sample preparation, cooling, testing and softening point detection in the above method is about 54h, which is a long cycle. The storage test of polymer modified asphalt takes a long time when entering and leaving the factory. During this period, the modified asphalt has been in hot storage, and the asphalt decays and the quality decreases.

[0003] The phase state of polymer modified asphalt can reflect the compatibility of modifier and asphalt. The microscopic phase structure of modifier changes with the development time of modified asphalt. As the development time increases, the phase state of modifier changes from point to strip, then to network structure and homogeneous structure. Modified asphalt becomes more and more stable with the change of phase state. Segregation is currently used to characterize the stability of modified asphalt. When asphalt segregates, the modifier and asphalt separate and the modifier floats.

[0004] The Chinese patent with publication number CN1493877A discloses a method for evaluating the storage stability of polymer modified asphalt. Through fluorescence microscope observation, if the phase state is two phases uniformly dispersed, the storage stability of the sample is unqualified, and if the phase state is one phase, the storage stability is qualified; however, the accuracy of this method in evaluating the storage stability of polymer modified asphalt is low, and there is a large error. The Chinese patent with publication number CN112129731A discloses a method for rapid detection of storage stability of polymer modified asphalt. The relationship between the fluorescence spectrum and segregation is established through a standard spectrum, and the fluorescence spectrum is compared with the standard spectrum to determine whether the segregation is qualified; however, this method makes qualitative judgments through empirical values, and there is a large error.

[0005] The phase state of modified asphalt is greatly affected by the type of base asphalt and the content of modifier. After the base asphalt produced by different crude oils is modified, its phase state changes greatly. The connection with segregation established only through standard spectra is highly restrictive. After the type of base asphalt is determined, the phase state formed by different modifier contents also varies greatly. When the modifier content is low, the polymer-asphalt system is a single-phase system; when the polymer dosage increases, phase separation occurs, which is manifested as the polymer phase distributed in the continuous phase of asphalt; as the polymer dosage continues to increase, a mutually interconnected network is formed, which is manifested as two continuous phases; as the polymer dosage continues to increase, the asphalt phase becomes a discontinuous phase distributed in the continuous phase of the polymer. Under the change of modifier content and base asphalt factors, there are large differences in the phase state changes of modified asphalt. In existing studies, the segregation situation is qualitatively judged by establishing standard spectra or by empirical values.

[0006] In summary, how to quantitatively analyze the phase state and establish a model between it and the separation, and the selected characteristic values ​​can accurately quantify the phase state of different modifier contents and the phase state of different matrix asphalts, so that the detection of modified asphalt separation can be more accurate, efficient and convenient, which has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide a method for detecting the storage stability of SBS modified asphalt, which can quantitatively analyze the phase conditions of different modifier contents and different matrix asphalt phases and establish a model between them, so as to make the detection of modified asphalt separation more accurate, efficient and convenient.

[0008] The present invention provides a method for detecting the storage stability of SBS modified asphalt, comprising the following steps:

[0009] a) Using SBS modified asphalt to prepare fluorescent samples and detecting the SBS modified asphalt phase content;

[0010] b) substituting the SBS modified asphalt phase content obtained in step a) into the data model of the relationship between phase content and segregation to obtain segregation data, thereby completing the detection of the storage stability of the SBS modified asphalt;

[0011] The data model of the relationship between phase content and segregation is:

[0012]

[0013] Among them, x is the phase content and y is the segregation index.

[0014] Preferably, the process of preparing the fluorescent sample in step a) is specifically as follows:

[0015] The SBS modified asphalt was stirred evenly and heated in an oven using the hot drop slide method to prepare the fluorescent sample.

[0016] Preferably, the process of preparing the fluorescent sample by heating in an oven using the hot drop slide method is specifically as follows:

[0017] After the SBS modified asphalt is stirred evenly, a drop of SBS modified asphalt is dropped on a glass slide with a glass rod. After cooling to room temperature, cover it with a coverslip and heat the sample in an oven. After cooling to room temperature again, a fluorescent sample is obtained for fluorescence observation.

[0018] Preferably, the oven temperature for heating the sample in the oven is 160° C. to 165° C., and the time is 1 min to 2 min.

[0019] Preferably, the process of detecting the SBS modified asphalt phase content in step a) is specifically as follows:

[0020] A fluorescence microscope is used to collect images of fluorescent samples to obtain fluorescent images; then the fluorescent images are processed and calculated using image processing software, and corresponding threshold parameters and appropriate tolerances are set according to the characteristics of the fluorescent images to obtain the phase content.

[0021] Preferably, the process of performing image acquisition is specifically as follows:

[0022] Turn on the microscope, fluorescent emitter, and computer to preheat the equipment; place the fluorescent sample on the stage and fix it, select the appropriate magnification to take pictures and save them.

[0023] Preferably, in order to reduce the test error, each fluorescent sample is imaged at a different position, and a total of 2 to 4 images are collected, and photographed and saved respectively.

[0024] Preferably, the suitable magnification is 30 to 50 times.

[0025] Preferably, the process of processing and calculating is specifically as follows:

[0026] Open the software, open the fluorescent image to be analyzed, set the field of view according to the image clarity, set the field of view size to 100 pixels in width and 100 pixels in height and save it, open the set field of view image, create a new phase, set the upper tolerance and lower tolerance according to the image situation, save and apply it, measure the area content of the second phase, and obtain the phase content.

[0027] Preferably, the method for establishing the data model of the relationship between phase content and segregation in step b) is specifically as follows:

[0028] The phase content data of different SBS modified asphalts are obtained through step a), and the segregation indexes of the above different SBS modified asphalts are detected, the relationship between the phase content and the segregation index is established, and a data model of the relationship between the phase content and the segregation is obtained.

[0029] The present invention provides a method for detecting storage stability of SBS modified asphalt, comprising the following steps: a) preparing a fluorescent sample using SBS modified asphalt, and detecting the phase content of the SBS modified asphalt; b) substituting the phase content of the SBS modified asphalt obtained in step a) into a data model of the relationship between phase content and segregation, obtaining segregation data, and completing the detection of storage stability of the SBS modified asphalt; the data model of the relationship between phase content and segregation is:

[0030]

[0031] Wherein, x is the phase content, and y is the segregation index. Compared with the prior art, the detection method provided by the present invention can quantitatively analyze the phase state of different modifier contents and different matrix asphalt phase states and establish a model between them and segregation, making the detection of modified asphalt segregation more accurate, efficient and convenient.

[0032] At the same time, the detection method provided by the present invention is applicable to various grades of SBS modified asphalt. According to the established data model, the separation data can be quickly obtained to improve the detection efficiency. Moreover, by adopting the above-mentioned rapid detection and separation method, during the preparation process of modified asphalt, process monitoring can also be carried out to control the development degree of modified asphalt and improve the quality of modified asphalt. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the fluorescence image of Example 1 of the present invention;

[0034] Figure 2 This is a phase content picture of Example 1 of the present invention;

[0035] Figure 3 This is the fluorescence image of Example 2 of the present invention;

[0036] Figure 4 This is a phase content picture of Example 2 of the present invention;

[0037] Figure 5 This is the fluorescence image of Example 3 of the present invention;

[0038] Figure 6 This is a phase content picture of Example 3 of the present invention. DETAILED DESCRIPTION

[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] The present invention provides a method for detecting the storage stability of SBS modified asphalt, comprising the following steps:

[0041] a) Using SBS modified asphalt to prepare fluorescent samples and detecting the SBS modified asphalt phase content;

[0042] b) substituting the SBS modified asphalt phase content obtained in step a) into the data model of the relationship between phase content and segregation to obtain segregation data, thereby completing the detection of the storage stability of the SBS modified asphalt;

[0043] The data model of the relationship between phase content and segregation is:

[0044]

[0045] Among them, x is the phase content and y is the segregation index.

[0046] The present invention firstly uses SBS modified asphalt to prepare a fluorescent sample and detects the phase content of the SBS modified asphalt. The present invention has no special restrictions on the SBS modified asphalt, and commercially available SBS modified asphalts of various grades well known to those skilled in the art and homemade SBS modified asphalts can be used.

[0047] In the present invention, the process of preparing the fluorescent sample is preferably specifically as follows:

[0048] The SBS modified asphalt was stirred evenly and heated in an oven using the hot drop slide method to prepare the fluorescent sample.

[0049] In the present invention, the process of preparing the fluorescent sample by heating in an oven using the hot drop slide method is preferably as follows:

[0050] After the SBS modified asphalt is stirred evenly, a drop of SBS modified asphalt is dropped on a glass slide with a glass rod. After cooling to room temperature, cover it with a coverslip and heat the sample in an oven. After cooling to room temperature again, a fluorescent sample is obtained for fluorescence observation.

[0051] In the present invention, the oven temperature for heating the sample in the oven is preferably 160° C. to 165° C., more preferably 163° C., and the time is 1 min to 2 min.

[0052] In the present invention, the process of detecting the SBS modified asphalt phase content is preferably as follows:

[0053] A fluorescence microscope is used to collect images of fluorescent samples to obtain fluorescent images; then the fluorescent images are processed and calculated using image processing software, and corresponding threshold parameters and appropriate tolerances are set according to the characteristics of the fluorescent images to obtain the phase content.

[0054] In the present invention, the process of performing image acquisition is preferably specifically as follows:

[0055] Turn on the microscope, fluorescent emitter, and computer to preheat the equipment; place the fluorescent sample on the stage and fix it, select the appropriate magnification to take pictures and save them.

[0056] In the present invention, in order to reduce the test error, it is preferred that each fluorescent sample is imaged at different positions, and a total of 2 to 4 images are collected, which are photographed and saved separately. It is more preferred that each fluorescent sample is imaged at different positions, and a total of 3 images are collected, which are photographed and saved separately.

[0057] In the present invention, the suitable magnification is preferably 30 to 50 times, more preferably 40 times; at the same time, a suitable exposure should also be selected during the photo-taking process, specifically based on visual judgment of the picture clarity, and the present invention has no special restrictions on this.

[0058] In the present invention, the process of processing and calculating is preferably specifically as follows:

[0059] Open the software, open the fluorescent image to be analyzed, set the field of view according to the image clarity, set the field of view size to 100 pixels in width and 100 pixels in height and save it, open the set field of view image, create a new phase, set the upper tolerance and lower tolerance according to the image situation, save and apply it, measure the area content of the second phase, and obtain the phase content.

[0060] After the SBS modified asphalt phase content is detected, the present invention substitutes the obtained SBS modified asphalt phase content into a data model of the relationship between phase content and segregation to obtain segregation data, thereby completing the detection of the storage stability of the SBS modified asphalt.

[0061] In the present invention, the data model of the relationship between phase content and segregation is preferably:

[0062]

[0063] Among them, x is the phase content and y is the segregation index.

[0064] In the present invention, the method for establishing the data model of the relationship between phase content and segregation is preferably as follows:

[0065] The phase content data of different SBS modified asphalts are obtained through step a), and the segregation indexes of the above different SBS modified asphalts are detected, the relationship between the phase content and the segregation index is established, and a data model of the relationship between the phase content and the segregation index is obtained; that is, in order to accurately quantify different phase conditions, the phase content is selected as the phase quantification value. The present invention adopts sample preparation (the sample to be tested is stirred evenly, and a hot drop slide method is adopted to prepare a fluorescent sample in a 163°C oven), sample testing (the fluorescent sample is imaged using a fluorescence microscope, and a suitable magnification and exposure are selected to take pictures and save them. In order to reduce the test error, each fluorescent sample is imaged at different positions, and a total of 3 images are collected, which are photographed and saved respectively), and calculation (pictures are taken using a microscope). The processing software processes and calculates the fluorescent image, sets corresponding threshold parameters according to the image characteristics, sets appropriate tolerances, obtains phase content) and models (establishes the relationship between phase content and segregation, and establishes a data model), and obtains a data model of the relationship between phase content and segregation that can quickly and accurately detect the segregation of SBS modified asphalt. According to the data model, the detection of modified asphalt segregation can be made more accurate, efficient and convenient; at the same time, the detection method provided by the present invention is applicable to various grades of SBS modified asphalt, and according to the established data model, the segregation data can be quickly obtained to improve the detection efficiency; and, by adopting the above-mentioned method for rapid detection of segregation, process monitoring can also be carried out during the preparation process of modified asphalt to control the degree of development of modified asphalt and improve the quality of modified asphalt.

[0066] The present invention provides a method for rapidly detecting the storage stability of SBS modified asphalt, which can also be said to be a method for rapidly detecting the segregation of SBS modified asphalt. According to an established data model, segregation data can be rapidly obtained to improve detection efficiency. Moreover, by adopting the rapid detection and segregation method, process monitoring can also be performed during the preparation of the modified asphalt to control the degree of development of the modified asphalt and improve the quality of the modified asphalt.

[0067] The present invention provides a method for detecting storage stability of SBS modified asphalt, comprising the following steps: a) preparing a fluorescent sample using SBS modified asphalt, and detecting the phase content of the SBS modified asphalt; b) substituting the phase content of the SBS modified asphalt obtained in step a) into a data model of the relationship between phase content and segregation, obtaining segregation data, and completing the detection of storage stability of the SBS modified asphalt; the data model of the relationship between phase content and segregation is:

[0068]

[0069] Wherein, x is the phase content, and y is the segregation index. Compared with the prior art, the detection method provided by the present invention can quantitatively analyze the phase state of different modifier contents and different matrix asphalt phase states and establish a model between them and segregation, making the detection of modified asphalt segregation more accurate, efficient and convenient.

[0070] At the same time, the detection method provided by the present invention is applicable to various grades of SBS modified asphalt. According to the established data model, the separation data can be quickly obtained to improve the detection efficiency. Moreover, by adopting the above-mentioned rapid detection and separation method, during the preparation process of modified asphalt, process monitoring can also be carried out to control the development degree of modified asphalt and improve the quality of modified asphalt.

[0071] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The raw materials used in the following examples of the present invention are all commercially available; in the following examples, the process of preparing the fluorescent sample is specifically as follows:

[0072] After the sample to be tested is stirred evenly, a drop of SBS modified asphalt is dropped on the glass slide with a glass rod. After cooling to room temperature, cover it with a cover glass, and bake the sample in an oven at 163°C for 1min to 2min. After cooling to room temperature, fluorescence observation is performed.

[0073] The specific process of detecting the modified asphalt phase content is as follows:

[0074] First, a fluorescence microscope was used to collect images of the fluorescent samples: the microscope, fluorescent emitter, and computer were turned on to preheat the equipment, the slide was placed on the stage and fixed, a magnification of 40 objective lens was selected for observation, and the focal length was adjusted to make the image clearer and save it. To reduce the test error, each fluorescent sample was imaged at different positions, and a total of 3 images were collected, which were photographed and saved respectively; then, the fluorescent images were processed and calculated using image processing software: the software was opened, the fluorescent image to be analyzed was opened, the field of view was set according to the clarity of the image, the field of view size was set to 100 pixels in width and 100 pixels in height and saved, the set field of view image was opened, a new phase was established, the upper tolerance and lower tolerance were set according to the image situation, and the phase content was saved and applied, and the second phase area content was determined to obtain the phase content;

[0075] The data model is:

[0076]

[0077] Among them, x is the phase content and y is the segregation index.

[0078] Example 1

[0079] 550g Haiyun No. 70 base asphalt, 7g aromatic oil and 22g 791H SBS were mixed and modified asphalt was prepared using the laboratory standard production plan. The mixture was developed for 40 minutes, and a fluorescent sample was prepared to detect the modified asphalt phase content. The segregation index was calculated using a data model.

[0080] Example 2

[0081] 550g Haiyun No. 70 base asphalt, 7g aromatic oil and 24.75g 791H SBS were mixed and modified asphalt was prepared using the laboratory standard production plan. The mixture was developed for 100min, and a fluorescent sample was prepared to detect the modified asphalt phase content. The segregation index was calculated using a data model.

[0082] Example 3

[0083] 550g Haiyun No. 70 base asphalt, 15.4g aromatic oil and 24.75g 791H SBS were mixed and modified asphalt was prepared using the laboratory standard production plan. The mixture was developed for 100min, and a fluorescent sample was prepared to detect the modified asphalt phase content. The segregation index was calculated using a data model.

[0084] Comparative Example 1

[0085] 550g of Haiyun No. 70 base asphalt, 7g of aromatic oil and 22g of 791H SBS were mixed, and modified asphalt was prepared using the laboratory standard production plan, and the segregation of the modified asphalt was tested.

[0086] Comparative Example 2

[0087] 550g of Haiyun No. 70 base asphalt, 7g of aromatic oil, and 24.75g of 791H SBS were mixed, and modified asphalt was prepared using the laboratory standard production plan, and the segregation of the modified asphalt was tested.

[0088] Comparative Example 3

[0089] 550 g of Haiyun No. 70 base asphalt, 15.4 g of aromatic oil, and 24.75 g of 791H SBS were mixed, and modified asphalt was prepared using the laboratory standard production plan, and the segregation of the modified asphalt was tested.

[0090] The properties of the modified asphalt materials obtained in Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3 were tested. The test results are shown in Table 1. The fluorescence microscope images are shown in Table 1. Figures 1 to 6 shown.

[0091] Table 1 Performance test results of modified asphalt materials obtained in Examples 1 to 3 and Comparative Examples 1 to 3

[0092] Test items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Phase content / % 36.70 40.71 41.63 / / / Calculate segregation / ℃ 24.6 12.7 7.8 / / / Detection segregation / ℃ / / / 23.7 11.9 7.6 Detection time 5min 5min 5min 54h 54h 54h

[0093] From Table 1 and Figures 1 to 6The following conclusions were drawn: the phase contents of Example 1, Example 2, and Example 3 were calculated to be 36.70%, 40.71%, and 41.63%, respectively; the corresponding segregations were calculated to be 24.6°C, 12.7°C, and 7.8°C, respectively, through the established data model; the segregation data of the comparative example were detected, and the segregation data obtained were 23.7°C, 11.9°C, and 7.6°C; therefore, the established data model had an extremely high accuracy rate; the segregation index detection period calculated by the established mathematical model was 5 minutes, while the traditional segregation index detection required 54 hours; therefore, the present invention provides a method for rapidly detecting the segregation of SBS modified asphalt; according to the established data model, the segregation data can be rapidly obtained to improve the detection efficiency; by using the rapid detection and segregation method provided by the present invention, during the preparation process of modified asphalt, process monitoring can also be performed to control the development degree of modified asphalt and improve the quality of modified asphalt.

[0094] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for detecting the storage stability of SBS modified asphalt, comprising the following steps: a) Using SBS modified asphalt to prepare fluorescent samples and detecting the SBS modified asphalt phase content; b) substituting the SBS modified asphalt phase content obtained in step a) into the data model of the relationship between phase content and segregation to obtain segregation data, thereby completing the detection of the storage stability of the SBS modified asphalt; The data model of the relationship between phase content and segregation is: Among them, x is the phase content, y is the segregation index; The method for establishing the data model of the relationship between phase content and segregation is specifically as follows: The phase content data of different SBS modified asphalts are obtained through step a), and the segregation indexes of the above different SBS modified asphalts are detected, the relationship between the phase content and the segregation index is established, and a data model of the relationship between the phase content and the segregation is obtained.

2. The detection method according to claim 1, characterized in that: The process of preparing the fluorescent sample in step a) is specifically as follows: The SBS modified asphalt was stirred evenly and heated in an oven using the hot drop slide method to prepare the fluorescent sample.

3. The detection method according to claim 2, characterized in that: The process of preparing the fluorescent sample by heating in an oven using the hot drop slide method is as follows: After the SBS modified asphalt is stirred evenly, a drop of SBS modified asphalt is dropped on a glass slide with a glass rod. After cooling to room temperature, cover it with a coverslip and heat the sample in an oven. After cooling to room temperature again, a fluorescent sample is obtained for fluorescence observation.

4. The detection method according to claim 3, characterized in that: The oven temperature for heating the sample in the oven is 160° C. to 165° C., and the time is 1 min to 2 min.

5. The detection method according to claim 1, characterized in that: The process of detecting the SBS modified asphalt phase content in step a) is specifically as follows: A fluorescence microscope is used to collect images of fluorescent samples to obtain fluorescent images; then the fluorescent images are processed and calculated using image processing software, and corresponding threshold parameters and appropriate tolerances are set according to the characteristics of the fluorescent images to obtain the phase content.

6. The detection method according to claim 5, characterized in that: The process of image acquisition is specifically as follows: Turn on the microscope, fluorescent emitter, and computer to preheat the equipment; place the fluorescent sample on the stage and fix it, select the appropriate magnification to take pictures and save them.

7. The detection method according to claim 6, characterized in that: In order to reduce the test error, each fluorescent sample was imaged at different positions, with a total of 2 to 4 images collected, which were photographed and saved separately.

8. The detection method according to claim 6, characterized in that: The suitable magnification is 30 to 50 times.

9. The detection method according to claim 5, characterized in that: The specific process of processing and calculating is as follows: Open the software, open the fluorescent image to be analyzed, set the field of view according to the image clarity, set the field of view size to 100 pixels in width and 100 pixels in height and save it, open the set field of view image, create a new phase, set the upper tolerance and lower tolerance according to the image situation, save and apply it, measure the area content of the second phase, and obtain the phase content.