A carbon halide tin battery
By using tin tetrachloride as the electrolyte and graphite, tin metal or tin compound embedded in halogen as materials in lithium-ion batteries, the problem of flammability of lithium-ion batteries is solved, and a non-flammable carbon halogen tin battery is realized, which improves the improvement of Energy density and charge and discharge power, and reduce material costs and safety risks.
Patent Information
- Application Number
- CN202211039642.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Lithium-ion batteries are prone to combustion accidents because the flammable solvent used and the release of oxygen from the positive electrode material at high temperatures intensifies combustion.
A carbon halogen tin battery is used, the electrolyte is tin tetrachloride, the positive electrode material is graphite embedded in halogen, and the negative electrode material is tin metal or tin compound, which avoids the existence of oxygen and hydrogen elements, and tin tetrachloride is used as the electrolyte.
It realizes a non-combustible battery, improves energy density and charge and discharge power, and the material is relatively cheap, safe and environmentally friendly, and can control thermal runaway in abnormal situations and reduce combustion risks.
Smart Images

Figure CN115172866B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a carbon halogen tin battery. Background Art
[0002] Lithium-ion batteries often catch fire. The media often reports fire accidents in electric vehicles, electric bicycles, and energy storage systems that use lithium-ion batteries. The reasons are: (1) The use of Class IA and B flammable solvents in the electrolyte ester (C x1 H x2 O x3 ), in abnormal cases, the electrolyte decomposes to form Class A and B flammable gases such as hydrocarbon gas (C x1 H x4 Once the battery is abused and an ignition source is generated, these Class A and B flammable substances will ignite, causing intense combustion. (2) Positive electrodes such as lithium cobalt oxide (LiCoO2), lithium nickel cobalt manganese (LiNi x1 Co x5 Mn 1-x1-x5 O2) and lithium iron phosphate (LiFePO4) powder release oxygen at high temperature, intensifying combustion. Summary of the invention
[0003] In view of this, an object of the present invention is to provide a carbon halogen tin battery. The carbon halogen tin battery provided by the present invention is not easy to burn.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] The present application provides a carbon halide tin battery, wherein the electrolyte of the battery is tin tetrachloride.
[0006] Preferably, the positive electrode material of the battery is halogen-embedded graphite.
[0007] Preferably, the halogen is at least one of Br, I and Cl.
[0008] Preferably, the molar ratio of the halogen to the carbon element in graphite is 1:2-30.
[0009] Preferably, the negative electrode material of the battery is tin metal or a tin compound.
[0010] Preferably, the tin compound is SnM p , M is a metal element or non-metal element that can accommodate tin, and the p value is 6-24.
[0011] Beneficial technical effects: The present invention provides a carbon halide tin battery, wherein the positive electrode, negative electrode and electrolyte of the battery do not contain oxygen and hydrogen elements, which are basically non-combustible elements and have good flame retardancy. The electrolyte SnCl4 is also an electrolyte, and no additional solution is required, which can improve energy density and charge and discharge power. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Schematic diagram of the structure of carbon halide tin battery;
[0013] 1- positive electrode sheet, 2- negative electrode sheet, 3- isolating film, 4- Cl - , 5-SnCl4, 6-Sn 4+ . DETAILED DESCRIPTION
[0014] The present application provides a carbon halide tin battery, wherein the electrolyte of the battery is tin tetrachloride.
[0015] In the present invention, the positive electrode material of the battery is halogen-embedded graphite, wherein the halogen is at least one of Br, I and Cl; the molar ratio of the halogen to the carbon element in the graphite is 1:2 to 30, more preferably 1:7 to 14; specifically, the molecular formula of the halogen-embedded graphite is C x A y Cl z or C x A y , the A is preferably Br or I, the molar ratio of the halogen to the carbon element in the graphite is a set ratio, which varies according to the depth of charge and discharge, for example, typical values are x=3.5, y=0.5, z=0.5.
[0016] In the present invention, the preparation method of the positive electrode material comprises: mixing graphite powder with a halogen element to obtain halogen-embedded graphite. In the present invention, the molar ratio of the graphite powder to the halogen element is preferably 2-30, more preferably 7-14.
[0017] The present invention coats the positive electrode material on both sides of the metal current collector, and then compresses, seals, and manufactures the pole lugs to obtain the positive electrode sheet. The present invention does not specifically limit the coating method, and a coating method well known to those skilled in the art can be selected to uniformly coat the positive electrode material on the current collector surface.
[0018] In the present invention, the negative electrode material of the battery is tin metal or tin compound, and the tin compound is preferably SnM p , wherein M is a metal element or non-metal element that can accommodate tin, and is preferably SnC p The p value is preferably 6-24, more preferably 6-12.
[0019] The present invention sequentially dries and dehumidifies the negative electrode material, calenders, cuts, and manufactures negative electrode tabs to obtain negative electrode sheets.
[0020] The present invention winds or stacks the positive electrode, the negative electrode and the isolation film to form a naked battery cell; tests the insulation of the naked battery cell, and puts normal products into a battery shell; injects the electrolyte SnCl4 in a dry environment to test the injection volume; performs formation charging and discharging according to a set process, and exhaust gas can be partially extracted during the formation, and then a sealed box is tested; and normal products are stored in a warehouse for shipment.
[0021] In the present invention, the working principle of the carbon halide tin battery is:
[0022] Positive 8C x A y +8z - -8ze - =8C x A y Cl z
[0023] Negative electrode 2zSn 4+ +8ze - =2zSn
[0024] or 2zSn 4+ +8ze - +(1-2z)SnM p1 =SnM p2
[0025] Electrolyte 2zSnCl4=2zSn 4+ +8z -
[0026] Overall reaction equation 8C x A y +8z - +2zSn 4+ =8C X A y Cl z +2zSn
[0027] or 8C x A y +8z - +2zSn 4+ +(1-2z)SnM p1 =8C X A y Cl z +SnM p2
[0028] Wherein A is Br or I, and x:y:z is the molar ratio of C, A and Cl in the carbon halide tin battery positive electrode material.
[0029] The working principle diagram of the carbon halide tin battery of the present invention is as follows: Figure 1 shown.
[0030] The carbon halogen tin battery positive electrode, negative electrode and electrolyte provided by the present invention do not contain oxygen and hydrogen elements, which are basically non-combustible elements, thus forming a battery that is not easy to burn.
[0031] Compared with the precious metals cobalt, nickel and lithium used in lithium-ion batteries, the carbon halide tin battery provided by the present invention uses graphite, tin metal and tin tetrachloride, which are much cheaper.
[0032] The electrolyte SnCl4 of the present invention is liquid in the working scenario and does not require additional solutions. It can improve the energy density and charging and discharging power and realize the fast charging function.
[0033] The tin metal in the carbon halide tin battery provided by the present invention can be used to make toothpaste shells, and the graphite can be used to make medical bandages for burns, both of which are non-toxic and environmentally friendly products; the electrolyte tin tetrachloride is moderately toxic, and will react when leaked into the environment, and its safety and environmental risks are controllable.
[0034] The present invention uses SnCl4 as electrolyte, halogen-embedded graphite as positive electrode material, and tin or tin compound as negative electrode material to form a battery. During the charge and discharge process, it is necessary to reasonably control side reaction substances such as Cl2, SnCl2, SnI2, SnI4, SnBr2, and SnBr4. An appropriate amount of chlorine gas Cl2 can prevent the liquid electrolyte SnCl4 from forming solid SnCl2, but an excessive amount will consume the liquid SnCl4; an appropriate amount of solid SnCl2, SnI2, SnI4, SnBr2, and SnBr4 can help form an interface coating layer of the negative electrode, and an excessive amount will cause a sharp drop in conductivity or even inability to conduct electricity.
[0035] In the present invention, the operating temperature of the battery is preferably 20-60°C, and the battery of the present invention can be normally charged and discharged within the operating temperature window; under abnormal circumstances, the temperature is used to control the thermal runaway of multiple batteries to reduce the intensity of the reaction, such as high temperature combustion causes the liquid electrolyte to gasify and reduce the battery's conductive power or even make it non-conductive; after impact and damage, the electrolyte leaks out or reacts with water to form gas decomposition, reducing the battery's conductive power or even making it non-conductive; a safety device for spraying low-temperature substances is provided, and in an emergency, the low-temperature substances are sprayed to freeze the liquid electrolyte into a solid and the tin metal is cooled and powdered, reducing the battery's conductive power or even making it non-conductive.
[0036] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0037] Example 1
[0038] 1) 3.5 mol of graphite powder and 0.5 mol of bromine are mixed to obtain a mixed raw material, and the mixed raw material is evenly coated on both sides of the metal current collector, and then pressed, sealed, and made into a tab to form a positive electrode sheet.
[0039] 2) Selecting metallic tin, drying and dehumidifying it, rolling it into a tin foil roll, slitting it into a reasonable width, manufacturing a negative electrode tab, and forming a negative electrode sheet.
[0040] 3) Select liquid SnCl4, dry and remove impurities in sequence, and use it as an electrolyte.
[0041] 4) Battery assembly
[0042] (a) Separate the positive electrode sheet, the separator, and the negative electrode sheet, and tape can be applied locally to increase insulation. Use lamination or winding technology to form a bare cell;
[0043] (b) Conduct insulation test and alignment test on bare cells;
[0044] (c) placing the bare battery cell in a battery casing;
[0045] (d) pouring tin tetrachloride electrolyte in a dry environment, and maintaining local vacuum exhaust during the pouring process;
[0046] (e) After the filling is completed, the battery is packaged to form a carbon halide tin battery;
[0047] (f) Carry out appearance inspection, sealing inspection and random inspection for alignment.
[0048] 5) Battery formation
[0049] (a) Performing the formation process of charging and discharging, and partially evacuating the gas; sealing after the charging and discharging is completed;
[0050] (b) Test battery size and sealing performance;
[0051] (c) Test battery electrical properties such as open circuit voltage, self-discharge rate, capacity, etc.
[0052] Example 2
[0053] 1) 3.5 mol of graphite powder and 0.5 mol of iodine are mixed to obtain a mixed raw material, and the mixed raw material is evenly coated on both sides of the metal current collector, and then pressed, sealed, and made into a tab to form a positive electrode sheet.
[0054] Steps 2 to 3) are exactly the same as in Example 1.
[0055] Example 3
[0056] The metal in step 2) is carbon-tin alloy SnC6, and the other steps are exactly the same as those in Example 1.
[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A carbon halide tin battery, characterized in that: The electrolyte of the battery is tin tetrachloride.
2. The battery according to claim 1, characterized in that The positive electrode material of the battery is halogen-intercalated graphite.
3. The battery according to claim 2, characterized in that The halogen is at least one of Br, I and Cl.
4. The battery according to claim 2 or 3, characterized in that: The molar ratio of the halogen to the carbon element in the graphite is 1:2-30.
5. The battery according to claim 1, characterized in that The negative electrode material of the battery is tin metal or tin compound.
6. The battery according to claim 5, characterized in that The tin compound is SnMp, M is a metal element or a non-metal element that can accommodate tin, and the value of p is 6-24.