A smelting device and method for improving the control accuracy of nitrogen content in high nitrogen steel
By designing the vacuum chamber and induction furnace crucible during the smelting process of high-nitrogen steel, and using the sealing cover and probe system to calculate the amount of supplementary nitrogen gas, the problem of low nitrogen content control accuracy was solved, and precise nitrogen content control of high-nitrogen steel was achieved, improving Improve smelting accuracy and reduce costs.
Patent Information
- Application Number
- CN202210749368.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-06-29
AI Technical Summary
It is difficult to stably control the nitrogen yield during the smelting process of high-nitrogen steel, resulting in low precision of nitrogen content control, which seriously restricts the promotion and application of high-nitrogen steel.
A smelting device including a vacuum chamber, induction furnace crucible, sealing cover and pressure and temperature probes was designed. By calculating and supplementing the amount of nitrogen gas, a nitrogen-increasing sealed space was formed to achieve precise control of nitrogen and ensure the nitrogen content in the molten steel. reach the target value.
It achieves precise control of the nitrogen content of high-nitrogen steel, improves smelting accuracy, has a simple structure, is easy to operate and has low cost.
Smart Images

Figure CN115183579B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of smelting, and in particular to a smelting device and method for improving the control accuracy of nitrogen content in high-nitrogen steel. Background Art
[0002] As one of the important alloying elements, nitrogen in high nitrogen steel can improve the mechanical properties of steel, such as improving yield strength, tensile strength, wear resistance and corrosion resistance, and these beneficial effects all depend on the nitrogen content in the steel. During the smelting process of high nitrogen steel, nitrogen is usually added to the molten steel in the form of nitrogen alloys. Due to the limitation of the content of alloying elements in the steel, it is impossible to obtain a high nitrogen content by adding nitrogen alloys. Therefore, the current method of nitrogen blowing is used to increase nitrogen in high nitrogen steel smelting. Due to the complexity and instability of smelting conditions, it is difficult to stably control the yield of nitrogen in molten steel, resulting in a very low control accuracy of nitrogen content in steel, resulting in large performance differences between batches of high nitrogen steel, which seriously restricts the promotion and application of high nitrogen steel. Up to now, the precise control of nitrogen content in high nitrogen steel smelting has always been a difficult problem in the industry. Therefore, how to accurately control the nitrogen content in the process of high nitrogen steel smelting has become a difficult problem that the industry needs to solve urgently. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a smelting device and method for improving the control accuracy of the nitrogen content of high nitrogen steel, so as to achieve the purpose of accurately controlling the nitrogen content of high nitrogen steel.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] A smelting device for improving the control accuracy of nitrogen content in high nitrogen steel comprises a vacuum chamber, an induction furnace crucible and a steel ingot mold; a sealing steel ring seat is arranged on the upper periphery of the induction furnace crucible, a sealing cover is arranged above the induction furnace crucible, the sealing cover is driven by a lifting and rotating mechanism and can be sealed and connected with the sealing steel ring seat, a pressure and temperature probe and a signal transmitter are arranged on the sealing cover, and a long-term temperature measuring probe is arranged on the side wall in the middle of the induction furnace crucible; a permeable brick is arranged at the bottom of the induction furnace crucible, and the permeable brick is connected to a nitrogen blowing pipe.
[0006] A vacuum chamber cover is arranged on the top of the vacuum chamber.
[0007] The inner cylindrical surface and the end surface of the sealing cover are provided with sealing grooves, and a high temperature resistant sealing rubber ring is installed in the sealing groove.
[0008] A smelting method for a high nitrogen steel smelting device, comprising the following steps:
[0009] 1) According to the composition and quality of the steel grade for smelting high nitrogen steel, weigh the scrap steel and alloy, and do not consider the nitrogen content when mixing; put the scrap steel and alloy into the crucible of the induction furnace, evacuate to below 20Pa, and keep evacuating, heat and melt the scrap steel and alloy, and take samples to detect the nitrogen content;
[0010] 2) Rotate the sealing cover to the top of the induction furnace crucible, lower the sealing cover and press it with the sealing steel ring seat to form a nitrogen-enhanced sealed space composed of the induction furnace crucible and the sealing cover;
[0011] 3) According to the crucible size and the weight of scrap steel and alloy, calculate the volume of the nitrogen-enhanced sealed space between the steel liquid surface and the sealing cover, and use L 空 express;
[0012] 4) Calculate the required nitrogen volume L according to the composition and weight of the high nitrogen steel grade to be smelted 氮 , calculated based on a 100% recovery rate, nitrogen is blown into the molten steel from the air-permeable bricks through a nitrogen blowing pipe;
[0013] 5) Induction heat the molten steel for 0 to 10 minutes, the nitrogen is fully dissolved in the molten steel, and the nitrogen-enhanced sealed space pressure P transmitted by the pressure and temperature probe and the signal transmitter is read. 空 and nitrogen-enhanced sealing space temperature T 空 , Long-term temperature probe steel liquid temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space, the nitrogen content in the molten steel, and the amount of nitrogen required to be replenished L 氮补 , press L 氮补 The amount of nitrogen replenishment;
[0014] 6) The molten steel 14 is inductively heated to the pouring temperature, the nitrogen is fully dissolved in the molten steel, and then the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter is read. 空 and nitrogen-enhanced sealing space temperature T 空 , Long-term temperature probe steel liquid temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space and the nitrogen content in the molten steel. If the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, fill the vacuum chamber with nitrogen until the pressure in the vacuum chamber is consistent with the pressure in the nitrogen-enhanced sealed space; if the difference between the nitrogen content in the molten steel and the target nitrogen content is greater than the required range, calculate the amount of nitrogen to be replenished again. 氮补 Re-blowing is performed until the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, and then nitrogen is filled into the vacuum chamber;
[0015] 7) Raise the sealing cover, tilt the induction furnace crucible, and inject the high nitrogen steel liquid into the ingot mold;
[0016] 8) After the steel ingot is cooled to room temperature, the vacuum chamber cover is opened and the steel ingot is taken out to obtain a high nitrogen steel ingot.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The smelting method of the invention can accurately control the nitrogen content of liquid steel of high nitrogen steel; the device has a simple structure and is easy to operate; and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a structural schematic diagram of the present invention.
[0020] Figure 2 It is a schematic diagram of the structure of the sealing cover.
[0021] In the figure: vacuum chamber 1, induction furnace crucible 2, vacuum chamber cover 3, sealing steel ring seat 4, sealing cover 5, lifting and rotating mechanism 6, pressure and temperature probe and signal transmitter 7, air-permeable brick 8, nitrogen blowing pipe 9, ingot mold 10, long-term temperature measuring probe 12, induction coil 13, molten steel 14, nitrogen-enhanced sealing space 15, sealing groove 16. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] like Figure 1-Figure 2 A smelting device for improving the control accuracy of nitrogen content in high nitrogen steel comprises a vacuum chamber 1, an induction furnace crucible 2 and a steel ingot mold 10; a sealing steel ring seat 4 is arranged on the upper periphery of the induction furnace crucible 2, a sealing cover 5 is arranged above the induction furnace crucible 2, the sealing cover 5 is driven by a lifting and rotating mechanism 6 and can be sealed and connected with the sealing steel ring seat 4, a pressure and temperature probe and a signal transmitter 7 are arranged on the sealing cover 5, and a long-term temperature measuring probe 12 is arranged on the side wall of the middle part of the induction furnace crucible 2; a permeable brick 8 is arranged at the bottom of the induction furnace crucible 2, and the permeable brick 8 is connected with a nitrogen blowing pipe 9.
[0024] A vacuum chamber cover 3 is provided on the top of the vacuum chamber 1 .
[0025] The inner cylindrical surface and the end surface of the sealing cover 5 are provided with a sealing groove 16 , and a high temperature resistant sealing rubber ring is installed in the sealing groove 16 .
[0026] The smelting method of the high nitrogen steel smelting device comprises the following steps:
[0027] 1) According to the composition and quality of the steel grade for smelting high nitrogen steel, weigh the scrap steel and alloy, and do not consider the nitrogen content when mixing; put the scrap steel and alloy into the crucible of the induction furnace, evacuate to below 20Pa, and keep evacuating, heat and melt the scrap steel and alloy, and take samples to detect the nitrogen content;
[0028] 2) Rotate the sealing cover 5 to the top of the induction furnace crucible, lower the sealing cover 5 and press it with the sealing steel ring seat 4 to form a nitrogen-enriched sealed space 15 composed of the induction furnace crucible 2 and the sealing cover 5;
[0029] 3) According to the crucible size and the weight of scrap steel and alloy, calculate the volume of the nitrogen-enhanced sealed space 15 between the steel liquid surface and the sealing cover, and use L 空 express;
[0030] 4) Calculate the required nitrogen volume L according to the composition and weight of the high nitrogen steel grade to be smelted 氮 , calculated based on a 100% recovery rate, nitrogen is blown into the molten steel from the nitrogen blowing pipe 9 through the air-permeable brick;
[0031] 5) Induction heat the molten steel for 0 to 10 minutes, the nitrogen is fully dissolved in the molten steel, and the nitrogen-enhanced sealed space pressure P transmitted by the pressure and temperature probe and the signal transmitter 7 is read. 空 and nitrogen-enhanced sealing space temperature T 空 , long-term temperature probe 12 molten steel temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space, the nitrogen content in the molten steel, and the amount of nitrogen required to be replenished L 氮补 , press L 氮补 The amount of nitrogen replenishment;
[0032] 6) The molten steel 14 is inductively heated to the pouring temperature, the nitrogen is fully dissolved in the molten steel, and then the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter 7 is read. 空 and nitrogen-enhanced sealing space temperature T 空 , long-term temperature probe 12 molten steel temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space and the nitrogen content in the molten steel. If the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, fill the vacuum chamber with nitrogen until the pressure in the vacuum chamber is consistent with the pressure in the nitrogen-enhanced sealed space 15; if the difference between the nitrogen content in the molten steel and the target nitrogen content is greater than the required range, calculate the amount of nitrogen to be replenished again L 氮补 Re-blowing is carried out until the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, and then nitrogen is filled into the vacuum chamber.
[0033] 7) Raise the sealing cover 5, tilt the induction furnace crucible, and inject the high nitrogen steel liquid into the ingot mold 10;
[0034] 8) After the steel ingot is cooled to room temperature, the vacuum chamber cover is opened and the steel ingot is taken out to obtain a high nitrogen steel ingot.
[0035] Example 1
[0036] The smelting method of the high nitrogen steel smelting device is used to prepare a 500kg steel ingot of marine Cr18Mn18 high nitrogen steel (nitrogen content target value: 0.80%, range ±0.0020%). The steps are:
[0037] 1) According to the composition and quality of Cr18Mn18 high nitrogen steel, weigh the scrap steel and alloy, and do not consider the nitrogen content when mixing. Put the scrap steel and alloy into the crucible 2 of the induction furnace, evacuate to 18Pa, and keep evacuating, heat and melt the scrap steel and alloy to 1570℃, and take samples to test the nitrogen content. According to the size of the crucible and the weight of the scrap steel and alloy, calculate the volume of the nitrogen-enhanced sealed space 15 between the steel liquid surface and the sealing cover 5, and use the symbol L 空 express;
[0038] 2) Operate the lifting and rotating mechanism 6 to rotate the sealing cover 5 to the top of the induction furnace crucible 2. Lower the sealing cover 5 and press it with the sealing steel ring seat 4 to form a nitrogen-enriched sealed space 15 composed of the induction furnace crucible 2 and the sealing cover 5;
[0039] 3) Calculate the required nitrogen volume L according to the composition and weight of the high nitrogen steel grade to be smelted 氮 , calculated based on a 100% recovery rate. Blow nitrogen into the molten steel through the nitrogen blowing pipe 9 and the air-permeable brick 8;
[0040] 4) Induction heating of molten steel for 3 minutes, nitrogen fully dissolved in the molten steel. The computer reads the nitrogen-enhanced sealed space pressure P transmitted by the pressure and temperature probe and signal transmitter 7. 空 =0.0812 MPa, nitrogen-enhanced sealing space temperature T 空 =1581℃, and long-term temperature probe 12 steel liquid temperature T 钢液 According to the above data, calculate the nitrogen quality in the nitrogen-enhanced sealed space, the nitrogen content in the molten steel, and the amount of nitrogen required to be replenished L 氮补 . Set the volume to L 氮补 Nitrogen is blown into the molten steel;
[0041] 5) The molten steel 14 is induction heated to a pouring temperature of 1590°C. The computer then reads the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter 7. 空 = 0.0817 MPa and nitrogen-enhanced sealing space temperature T 空 , and long-term temperature probe 12 steel liquid temperature T 钢液 , calculate the nitrogen mass in the nitrogen-enhanced sealed space and the nitrogen content in the molten steel based on the above data. The nitrogen content in the molten steel is calculated to be 0.8003%, which is within the required composition range. Fill the vacuum chamber 1 with nitrogen until the pressure is consistent with that in the nitrogen-enhanced sealed space 15;
[0042] 6) Operate the lifting and rotating mechanism 6 to raise the sealing cover 5, tilt the induction furnace, and inject the high nitrogen steel liquid into the ingot mold 10;
[0043] 7) After the steel ingot is cooled to room temperature, the vacuum chamber cover 3 is opened and the steel ingot is taken out to obtain a Cr18Mn18 high nitrogen steel ingot.
[0044] Sampling and testing of the chemical composition of the steel ingot showed a nitrogen content of 0.8002%, with a deviation of 0.0002% from the target value. The composition accuracy is much higher than that of the traditional smelting method (the nitrogen content control accuracy of this type of steel using the traditional smelting method is ±0.0090%).
[0045] Example 2
[0046] The smelting method of the high nitrogen steel smelting device, the preparation of 1000kg steel ingot of high nitrogen 316L stainless steel welding wire steel (nitrogen content target value: 0.97%, range ±0.0025%), the steps are:
[0047] 1) According to the composition and mass (M) of high nitrogen 316L stainless steel welding wire steel, weigh the scrap steel and alloy, and do not consider the nitrogen content when mixing. Put the scrap steel and alloy into the crucible 2 of the induction furnace, evacuate to below 20Pa and keep evacuating, heat and melt the scrap steel and alloy to 1536℃, and take samples to test the nitrogen content. According to the size of the crucible and the weight of the scrap steel and alloy, calculate the volume of the nitrogen-enhanced sealed space 15 between the steel liquid surface and the sealing cover 5, and use the symbol L 空 express;
[0048] 2) Operate the lifting and rotating mechanism 6 to rotate the sealing cover 5 to the top of the induction furnace crucible 2. Lower the sealing cover 5 and press it with the sealing steel ring seat 4 to form a nitrogen-enriched sealed space 15 composed of the induction furnace crucible 2 and the sealing cover 5;
[0049] 3) Calculate the required nitrogen volume L according to the composition and weight of the high nitrogen steel grade to be smelted 氮 , calculated based on a 100% recovery rate. Blow nitrogen into the molten steel through the nitrogen blowing pipe 9 and the air-permeable brick 8;
[0050] 4) Induction heating of molten steel for 3 minutes, nitrogen fully dissolved in the molten steel. The computer reads the nitrogen-enhanced sealed space pressure P transmitted by the pressure and temperature probe and signal transmitter 7. 空 = 0.0788 MPa and temperature T 空 =1551℃, and long-term temperature probe 12 steel liquid temperature T 钢液 According to the above data, calculate the nitrogen quality in the nitrogen-enhanced sealed space, the nitrogen content in the molten steel, and the amount of nitrogen required to be replenished L 氮补 . Set the volume to L 氮补 Nitrogen is blown into the molten steel;
[0051] 5) The molten steel 14 is induction heated to a pouring temperature of 1590°C. The computer then reads the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter 7. 空= 0.0813 MPa and temperature T 空 Data, and long-term temperature probe 12 molten steel temperature data T 钢液 , calculate the nitrogen mass in the nitrogen-enhanced sealed space and the nitrogen content in the molten steel based on the above data. The nitrogen content in the molten steel is calculated to be 0.9704%, which is within the required composition range. Fill the vacuum chamber of the induction furnace with nitrogen until the pressure is consistent with that in the nitrogen-enhanced sealed space 15;
[0052] 6) Operate the lifting and rotating mechanism 6 to raise the sealing cover 5, tilt the induction furnace, and inject the high nitrogen steel liquid into the ingot mold 10;
[0053] 7) After the steel ingot is cooled to room temperature, the vacuum chamber cover is opened and the steel ingot is taken out to obtain a high nitrogen 316L stainless steel welding wire steel ingot.
[0054] Sampling and testing of the chemical composition of the steel ingot showed a nitrogen content of 0.9703%, with a deviation of 0.0003% from the target value. The composition accuracy is much higher than that of the traditional smelting method (the nitrogen content control accuracy of this type of steel using the traditional smelting method is ±0.0100%).
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A smelting method for a smelting device for improving the control accuracy of nitrogen content in high nitrogen steel, characterized in that: The smelting device comprises a vacuum chamber, an induction furnace crucible, and a steel ingot mold; a sealing steel ring seat is arranged on the upper outer periphery of the induction furnace crucible, a sealing cover is arranged above the induction furnace crucible, the sealing cover is driven by a lifting and rotating mechanism to be sealed and connected with the sealing steel ring seat, a pressure and temperature probe and a signal transmitter are arranged on the sealing cover, and a long-term temperature measuring probe is arranged on the side wall of the middle part of the induction furnace crucible; a permeable brick is arranged at the bottom of the induction furnace crucible, and the permeable brick is connected to a nitrogen blowing pipe; the smelting method comprises the following steps: 1) According to the composition and quality of the steel grade for smelting high nitrogen steel, weigh the scrap steel and alloy, and do not consider the nitrogen content when mixing; put the scrap steel and alloy into the crucible of the induction furnace, evacuate to below 20Pa, and keep evacuating, heat and melt the scrap steel and alloy, and take samples to detect the nitrogen content; 2) Rotate the sealing cover to the top of the induction furnace crucible, lower the sealing cover and press it with the sealing steel ring seat to form a nitrogen-enhanced sealed space composed of the induction furnace crucible and the sealing cover; 3) According to the crucible size and the weight of scrap steel and alloy, calculate the volume of the nitrogen-enhanced sealed space between the steel liquid surface and the sealing cover, and use L 空 express; 4) Calculate the required nitrogen volume L according to the composition and weight of the high nitrogen steel grade to be smelted 氮 , calculated based on a 100% recovery rate, nitrogen is blown into the molten steel from the air-permeable bricks through a nitrogen blowing pipe; 5) Induction heat the molten steel for 0 to 10 minutes, the nitrogen is fully dissolved in the molten steel, and the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter is read. 空 and nitrogen-enhanced sealing space temperature T 空 , Long-term temperature probe steel liquid temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space, the nitrogen content in the molten steel, and the amount of nitrogen required to be replenished L 氮补 , press L 氮补 The amount of nitrogen replenishment; 6) The molten steel is induction heated to the pouring temperature, the nitrogen is fully dissolved in the molten steel, and then the nitrogen-enhanced sealing space pressure P transmitted by the pressure and temperature probe and the signal transmitter is read. 空 and nitrogen-enhanced sealing space temperature T 空 , Long-term temperature probe steel liquid temperature T 钢液 , calculate the nitrogen quality in the nitrogen-enhanced sealed space and the nitrogen content in the molten steel. If the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, fill the vacuum chamber with nitrogen until the pressure in the vacuum chamber is consistent with the pressure in the nitrogen-enhanced sealed space; if the difference between the nitrogen content in the molten steel and the target nitrogen content is greater than the required range, calculate the amount of nitrogen to be replenished again. 氮补 Re-blowing is performed until the difference between the nitrogen content in the molten steel and the target nitrogen content is within the required range, and then nitrogen is filled into the vacuum chamber; 7) Raise the sealing cover, tilt the induction furnace crucible, and inject the high nitrogen steel liquid into the ingot mold; 8) After the steel ingot is cooled to room temperature, open the vacuum chamber cover, take out the steel ingot, and obtain a high nitrogen steel ingot.
2. The smelting method of a smelting device for improving the control accuracy of nitrogen content in high nitrogen steel according to claim 1, characterized in that: A vacuum chamber cover is arranged on the top of the vacuum chamber.
3. The smelting method of a smelting device for improving the control accuracy of nitrogen content in high nitrogen steel according to claim 1, characterized in that: The inner cylindrical surface and the end surface of the sealing cover are provided with sealing grooves, and a high temperature resistant sealing rubber ring is installed in the sealing groove.
Citation Information
Cited By
Method for stably controlling nitrogen content in steel by adopting vacuum induction furnace
CN119464902A