A high-activity high-purity ferric hydroxide, preparation method and application in the synthesis of ferric p-toluenesulfonate

By treating polymerized ferric sulfate in an alkali solution to prepare highly active and high-purity amorphous ferric hydroxide, and reacting with p-toluenesulfonic acid, the low production efficiency and cost of high-purity ferric p-toluenesulfonate in the existing technology are solved. High problem to improve the performance of solid aluminum capacitors.

CN115196684BActive Publication Date: 2024-10-01WUHAN HISPRING TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210877363.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-25
Publication Date
2024-10-01
Estimated Expiration
2042-07-25

AI Technical Summary

Technical Problem

The production efficiency of high-purity ferric p-toluenesulfonate in the existing technology is low, the cost of raw materials is high, and the activity and purity of ferric hydroxide are insufficient, which affects the quality and market competitiveness of solid aluminum capacitors.

Method used

Polymeric ferric sulfate is slowly dropped into alkali solution and frozen, then heated, filtered and dried to prepare highly active and high-purity amorphous ferric hydroxide, and reacted with p-toluenesulfonic acid to obtain high purity through closed shaking and filtration. Iron p-toluenesulfonate.

Benefits of technology

It improves the activity and purity of ferric hydroxide, reduces the preparation cost of ferric p-toluenesulfonate, reduces the impurity content, and improves the conductivity and product performance of solid aluminum capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115196684B_ABST
    Figure CN115196684B_ABST
Patent Text Reader

Abstract

The invention discloses a high-activity and high-purity iron hydroxide, a preparation method and an application of the iron hydroxide in the synthesis of ferric p-toluenesulfonate. The preparation method of the iron hydroxide comprises the following steps: generating a ferric hydroxide colloid from polyferric sulfate (PFS) under alkaline conditions, desorbing impurities by quenching the colloid to remove the adsorption of impurities, and then freeze-drying the water-containing iron hydroxide solid to remove moisture to prepare a high-activity and high-purity amorphous iron hydroxide solid; the iron hydroxide can be used to prepare high-purity ferric p-toluenesulfonate, and further to prepare a cathode material for a solid aluminum capacitor, which has a low impurity content, can reduce the equivalent series resistance of the solid capacitor, and improve the conductivity, and has a significant advantage in improving the performance parameters of the terminal product when applied to a solid aluminum capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-purity ferric hydroxide preparation, and more specifically to high-activity high-purity ferric hydroxide, a preparation method and application in synthesizing ferric p-toluenesulfonate. Background Art

[0002] As a capacitor product with good growth potential, polymer solid aluminum capacitor has good application prospects. The biggest difference between it and ordinary capacitors (i.e. liquid aluminum electrolytic capacitors) is that different dielectric materials are used. The cathode material of liquid aluminum capacitors is electrolyte, and the conduction method is ionic conduction; while the cathode material of solid polymer aluminum capacitors is conductive polymer, and the conduction method is electronic conduction. Its conductivity is about 10,000 times that of ordinary electrolytes. This material will not react with aluminum, and will not explode after power is turned on; at the same time, it is a solid product, so there is naturally no bursting due to thermal expansion. Solid polymer aluminum capacitors overcome performance defects such as low conductivity and leakage, and have the advantages of high frequency and low impedance, high ripple current resistance, good transient response characteristics, excellent temperature-frequency characteristics, good moisture resistance, small size, long life, safety and reliability, and suitable for surface mounting.

[0003] Solid electrolyte made of high-purity ferric p-toluenesulfonate solution is the core of solid polymer aluminum capacitors. After Bayer invented the conductive compound 3,4-ethylenedioxythiophene (EDOT for short), ferric p-toluenesulfonate has been widely recognized as an effective oxidant and polymerization driving material for EDOT. It is mainly used to manufacture solid polymer capacitors, conductive binders for lithium iron phosphate positive electrode materials of lithium batteries, electronic circuit boards and organic light-emitting diodes. Ferric p-toluenesulfonate is used as an oxidant and dopant to oxidize EDOT into PEDOT polymer with excellent conductive properties, which is used to manufacture conductive cathodes for solid electrolytic capacitors. The electrolytic capacitors made from it have stable performance and a service life of more than 10 years, far exceeding liquid electrolyte electrolytic capacitors. Due to the insufficient purity and high price of ferric p-toluenesulfonate produced by domestic manufacturers, the competitiveness of solid aluminum capacitor products is seriously affected. Aluminum capacitor manufacturers are eager to have higher purity and lower price conductive polymer driving materials to improve the quality, cost performance and market competitiveness of solid aluminum capacitors.

[0004] Most of the methods for synthesizing ferric p-toluenesulfonate that have been publicly reported at home and abroad have extremely low production efficiency, extremely high raw material cost consumption, and the produced ferric p-toluenesulfonate has high water content and high chloride ion, sulfate or nitrate ion content. Chloride ions can strongly corrode the electrolytic aluminum oxide film, which has a great impact on the leakage current of solid electrolytic capacitors. Nitrates are easy to migrate in polymerized PEDOT conductive materials, which has a great impact on the corrosion of the dielectric film of solid capacitors and shortens the high-temperature service life. Sulfate ions can corrode aluminum foil and seriously affect the product life. Sulfate ions produce ultra-fine precipitates of barium sulfate with free barium ions. It is difficult to remove the barium sulfate precipitates by ordinary filtration, which seriously affects the product purity and production efficiency.

[0005] Chinese patent document CN107827785A discloses a method for synthesizing ferric p-toluenesulfonate, which uses ferric sulfate and sodium hydroxide to react to generate ferric hydroxide, and then conventionally reduces the pressure to filter the ferric hydroxide. This process contains a high impurity content in the ferric hydroxide, and the filtration takes a very long time, which seriously affects the industrial efficiency. In addition, the reaction activity of ferric hydroxide and p-toluenesulfonic acid in aqueous solution is very low, resulting in a low yield and a high impurity content.

[0006] Chinese patent document CN102911089A discloses a method for preparing ferric p-toluenesulfonate and its solution, which uses ammonium ferric sulfate to react with sodium hydroxide to generate ferric hydroxide, and then filtrates the ferric hydroxide by hanging and drying. The impurity content is higher, and the product yield and purity are not further described. In addition, the crystallization method is agglomeration, and the product and impurities are not separated.

[0007] Chinese patent document CN104250220A discloses a method for preparing high-purity ferric p-toluenesulfonate, which directly skips the ferric hydroxide preparation process. It uses ferric hydroxide as a raw material to react with p-toluenesulfonic acid to prepare ferric p-toluenesulfonate. The product yield and purity are not further described. In fact, the ferric hydroxide production process consumes a lot of raw material costs and energy.

[0008] Chinese patent document CN101973913A discloses a clean synthesis method of high-purity iron p-toluenesulfonate, which uses high-cost raw materials and uses iron nitrate as the iron source. Nitrate ions can exist in various solvents and are difficult to remove. Nitrate ions are easy to migrate in polymerized PEDOT conductive materials, which has a great influence on the corrosion of the dielectric film of solid capacitors and shortens the high-temperature service life. There is no further description of the product yield and purity.

[0009] Therefore, it is necessary to propose a method for preparing high-activity and high-purity iron hydroxide for synthesizing high-purity iron p-toluenesulfonate, so as to promote its application in the preparation of solid-state aluminum capacitor cathode material products and improve market competitiveness. Summary of the invention

[0010] In order to overcome the above-mentioned defects of the prior art, the first object of the present invention is to provide a method for preparing high-activity and high-purity iron hydroxide, so as to solve the defects of the prior art that the iron hydroxide has low activity and purity, which affects the quality of downstream products; the second object of the present invention is to provide a method for preparing iron p-toluenesulfonate using the iron hydroxide to improve the purity of iron p-toluenesulfonate; the third object of the present invention is to provide the application of the above-mentioned iron p-toluenesulfonate in the synthesis of iron p-toluenesulfonate and the application in the preparation of solid aluminum capacitors.

[0011] In view of this, the technical solution of the present invention is as follows:

[0012] A method for preparing high-activity and high-purity ferric hydroxide comprises the following steps:

[0013] S1. Slowly add the polyferric sulfate solution to the alkaline solution until the pH value is 7.0-7.5;

[0014] S2. Freeze the system obtained in step S1 at -20~-50°C for 1~5h, then heat to 10~38°C and stir;

[0015] S3. The system obtained in step S2 is filtered, washed with water, and then freeze-dried to obtain high-activity and high-purity iron hydroxide.

[0016] In a preferred embodiment, the iron content of the polyferric sulfate is 19-23wt%.

[0017] In a preferred embodiment, the step S3 is filtered under a pressure of 0.1-0.3 MPa.

[0018] In a preferred embodiment, the step S3 is freeze-dried at 0.1-0.35 mbar and -20-5°C.

[0019] In one embodiment of the present invention, the ferric hydroxide obtained by the above-mentioned preparation method has Figure 1 The X-ray diffraction pattern shown has no diffraction peaks and the iron hydroxide is in an amorphous state.

[0020] A method for preparing ferric p-toluenesulfonate comprises adding p-toluenesulfonic acid monohydrate and ferric hydroxide solid in a molar ratio of 3:1 into a closed oscillating reaction shaker, mixing and oscillating at 105-120° C. for 16-24 hours, filtering, and taking the filtrate for crystallization to obtain ferric p-toluenesulfonate; the ferric hydroxide is obtained by the preparation method described above.

[0021] In a preferred embodiment, 2-3 times the amount of pure water is added to the system obtained after the oscillation reaction, stirred at 65-95° C. for 30-60 min to dissolve, and then filtered.

[0022] In a preferred embodiment, the p-toluenesulfonic acid monohydrate is prepared by mixing industrial p-toluenesulfonic acid with 1-3% by weight of barium hydroxide at 40-75° C., stirring for 2-5 hours, adding lignin, filtering, and crystallizing.

[0023] In a preferred embodiment, the filtrate is heated to 75-95° C. under a negative pressure of 0.085-0.1 MPa for concentration and crystallization.

[0024] The present invention also provides the use of the iron p-toluenesulfonate obtained by the preparation method in preparing a cathode material for a solid aluminum capacitor. The prepared cathode material has a low impurity content, can reduce the equivalent series resistance of the solid capacitor, and improve the conductivity.

[0025] Compared with the prior art, the beneficial effects of the present invention include but are not limited to:

[0026] The invention uses colloid produced by polyferric sulfate in alkaline solution to remove the colloidal adsorption under the condition of sudden cooling, then heats up, filters and washes to obtain ferric hydroxide hydrate, and after freeze-drying, amorphous high-purity ferric hydroxide can be obtained. The amorphous ferric hydroxide particles are fine and non-crystalline, and have good contact area and reaction activity when reacting with other substances.

[0027] The invention uses the amorphous high-purity ferric hydroxide and p-toluenesulfonic acid to prepare the p-toluenesulfonic acid ferric salt, which has high purity, sulfate ions can be reduced to below 10 ppm, and has high yield, thereby effectively reducing the preparation cost.

[0028] The solid aluminum capacitor cathode material prepared by the iron p-toluenesulfonate of the present invention has low impurity content, can reduce the equivalent series resistance of the solid capacitor, and improve the conductivity. When applied to solid aluminum capacitors, it has obvious advantages over existing technologies in improving the performance parameters of terminal products. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The XRD diagram of the solid iron hydroxide obtained by the preparation method of the present invention.

[0030] Figure 2 The following is a comparison diagram of XRD of different iron hydroxide solids of the present invention.

[0031] Figure 3 This is a SEM comparison of iron hydroxide prepared by the method of the present invention and comparative example 1.

[0032] Figure 4 These are SEM images of iron hydroxide of Comparative Examples 4 and 5 of the present invention.

[0033] Figure 5 The DSC thermodynamic diagram of p-toluenesulfonic acid monohydrate of the present invention is shown in FIG.

[0034] Figure 6 This is the DSC-TG diagram of p-toluenesulfonic acid monohydrate of the present invention.

[0035] Figure 7 It is the SEM picture of ferric p-toluenesulfonate of the present invention.

[0036] Figure 8 It is the DSC thermodynamic diagram of iron p-toluenesulfonate of the present invention.

[0037] Fig. 9 The figure is a SEM image of the ethanol solution of iron p-toluenesulfonate of the present invention.

[0038] Fig.10 The figure is the XRD diagram of the iron p-toluenesulfonate ethanol solution of the present invention. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] In order to solve the problems of high impurity content and low yield of ferric p-toluenesulfonate prepared by the prior art, it is necessary to start from the source and study a new path for preparing ferric hydroxide. Amorphous solids are also called amorphous bodies. The arrangement of atoms or molecules inside them is not periodic, and they are distributed randomly like liquids. They are a kind of non-crystalline solid. It has macroscopic uniformity, and this uniformity comes from the statistical law of disordered distribution of atoms; physical properties generally do not change with the measurement direction, which is called isotropy; it cannot spontaneously form a polyhedral shape; it has no fixed melting point; due to the non-periodic structure, it cannot produce a diffraction effect on X-rays. Considering the high activity that amorphous ferric hydroxide may have, it is theoretically advantageous to prepare amorphous ferric hydroxide to improve the activity and then use it to prepare ferric p-toluenesulfonate.

[0041] Polyferric sulfate is a commonly used inorganic polymer flocculant. It is a light yellow amorphous resin. It is a good choice for preparing amorphous ferric hydroxide solid. However, its strong adsorption defect will adsorb a large amount of impurities, affecting the purity of the product. In the process of researching and designing the preparation route, how to remove or avoid the introduction of impurities becomes the key point to be overcome.

[0042] The following raw materials are mainly used in the following implementations of the present invention:

[0043] Polyferric sulfate ([Fe2(OH) n (SO4) 3-n / 2 ]m ): Industrial grade, purity ≥98%;

[0044] Sodium hydroxide: industrial grade, purity ≥99%;

[0045] p-Toluenesulfonic acid: industrial grade, purity ≥98%;

[0046] Barium hydroxide: industrial grade, purity ≥98%;

[0047] Ethanol: reagent grade, content ≥99%;

[0048] 3,4-Ethylenedioxythiophene (EDOT): industrial grade, purity ≥98%.

[0049] In one embodiment of the present invention, the method for preparing high-activity high-purity ferric hydroxide comprises the following steps:

[0050] 1) Slowly add the polyferric sulfate solution into the alkaline solution until the pH value is 7.0-7.5;

[0051] 2) Freeze the colloidal solution obtained in step 1) at -20~-50℃ for 1~5h to remove the colloidal adsorption, then heat it to 10~38℃ and stir it for 5~30min;

[0052] 3) The system obtained in step 2) is filtered, washed with water, and then freeze-dried to remove water to obtain a high-activity and high-purity ferric hydroxide solid.

[0053] The XRD pattern of the high-activity iron hydroxide solid obtained by the above preparation method is as follows: Figure 1 As shown, SEM Figure 3 As shown in A, the sample iron hydroxide is amorphous iron hydroxide and there is no diffraction peak after testing and analysis. It can be judged that amorphous iron hydroxide has high activity and high reactivity. Compared with iron hydroxide crystals prepared by conventional methods, amorphous iron hydroxide solids have good contact area and reactivity.

[0054] In a preferred embodiment, a polyferric sulfate having an iron content of 19-23 wt% is selected; an alkali solution having a concentration of 10-40 wt%, such as sodium hydroxide, potassium hydroxide or ammonia water, is selected as the alkali solution and a 10-30 wt% aqueous solution of polyferric sulfate is added dropwise to the target pH value, and the molar ratio of iron element to hydroxide ion is controlled to be 1:3-3.5, preferably 1:3.01.

[0055] In a preferred embodiment, the filtrate obtained in step 3) is filtered under a pressure of 0.1-0.3 MPa, and the filter cake is replaced and washed 2-3 times with an equal amount of pure water from the filtrate to obtain a solid aqueous ferric hydroxide mixture (with a water content of 20-50 wt%), and the obtained solid aqueous ferric hydroxide mixture is then freeze-dried at 0.1 mbar-0.35 mbar and -20-5°C to remove moisture to obtain a high-activity and high-purity ferric hydroxide solid.

[0056] In another embodiment of the present invention, the method for preparing ferric p-toluenesulfonate comprises the following steps:

[0057] Purification of industrial p-toluenesulfonic acid: Add an equal amount of pure water to industrial p-toluenesulfonic acid to dissolve it, then add 1% to 3% by weight of barium hydroxide (the specific weight added is based on the amount of sulfate impurities in the p-toluenesulfonic acid), stir at 40 to 75°C for 2 to 5 hours, add lignin and filter, evaporate the filtrate to dryness to obtain high-purity p-toluenesulfonic acid solid containing crystal water;

[0058] Step 1) The DSC thermodynamic diagram of the prepared solid p-toluenesulfonic acid containing crystal water is as follows: Figure 5 As shown: There is obvious heat absorption phenomenon around 100℃. Figure 6 The DSC-TG graph shown shows that the weight loss in the plateau is -10.33% (mass content), which is consistent with the weight of p-toluenesulfonic acid containing one crystal water after dehydration. The p-toluenesulfonic acid content is 90.3-90.6wt% and the crystal water mass content is 9.4-9.7wt%, so it is determined that the substance is p-toluenesulfonic acid crystals containing monohydrate.

[0059] Preparation of ferric p-toluenesulfonate: p-toluenesulfonic acid monohydrate and the obtained high-purity active ferric hydroxide solid are added in a molar ratio of 3:1 into a closed oscillating reaction shaker, and mixed and oscillated at a constant temperature of 105-120°C for 16-24h;

[0060] Purification: Add 2-3 times amount of pure water to the ferric p-toluenesulfonate and unreacted impurities, stir at 65-95℃ for 30-60min to dissolve, wait until room temperature and filter, the filtrate is the ferric p-toluenesulfonate aqueous solution;

[0061] Crystallization: the filtrate of the aqueous solution of ferric p-toluenesulfonate is decompressed by 0.085-0.1 MPa and heated to 75-95°C, the aqueous solution of ferric p-toluenesulfonate is concentrated to a content of 50-65wt% of ferric p-toluenesulfonate, a large amount of p-toluenesulfonic acid flaky crystals are precipitated, and centrifugation is performed to obtain a filter cake of high-purity hydrous ferric p-toluenesulfonate flaky crystals; the ferric p-toluenesulfonate flaky crystals are decompressed by 0.085-0.1 MPa and dried at a constant temperature of 165-195°C for 4-10 hours to obtain a solid finished product.

[0062] The solid SEM image of the product ferric p-toluenesulfonate obtained by the above preparation method is as follows Figure 7 As shown, it can be seen that the crystal morphology is obvious. The prepared crystals were analyzed by DSC thermodynamics as shown in Figure 8 As shown, the crystals are obviously different from the DSC thermodynamic diagram of p-toluenesulfonic acid, so the substance is determined to be iron p-toluenesulfonate.

[0063] In another embodiment of the present invention, the obtained ferric toluenesulfonate solid is cooled to room temperature and then ethanol is added to dissolve it to prepare a ferric toluenesulfonate-ethanol solution with a mass content of 50%. The water content, chloride ion and iron ion content in the solution are respectively detected. The water content is less than 0.26%, the chloride ion is not detected, and the iron ion content is 5%. The SEM and XRD patterns of the ethanol solution sample of ferric toluenesulfonate are as follows: Fig. 9 , Fig.10 As shown: Fig. 9 (A: 100 μm, B: 20 ​​μm) No crystalline structure was found. Fig.10 No diffraction peaks appear in the chromatogram, so there are no unreacted iron hydroxide crystals, no iron oxide crystals generated by decomposition, and no other crystalline impurities.

[0064] When used, the iron p-toluenesulfonate-ethanol solution is mixed with 3,4-ethylenedioxythiophene (EDOT for short), prepolymerized at room temperature for 2 hours, then impregnated with capacitor aluminum foil, cured at 110°C, and dried to prepare a specific solid aluminum capacitor cathode material. The conductivity of the cathode material is measured to be greater than 1269S / cm, and the ESR of the solid capacitor is less than 3.5mΩ.

[0065] Preferred preparation examples and embodiments of the present invention are as follows:

[0066] Preparation Example 1

[0067] Take polyferric sulfate with an iron content of 19wt% to prepare a polyferric sulfate solution with a concentration of 10wt%, prepare a sodium hydroxide solution according to the molar ratio of iron to hydroxide ion of 1:3.01, add the polyferric sulfate solution dropwise to the 10wt% sodium hydroxide solution, stir to fully form a colloid, and measure the pH to be 7.0. The colloid is placed in a cold trap and quickly frozen to -50℃ for 1 hour, then heated to 38℃ and stirred for 5 minutes, filtered at a pressure of 0.1MPa, and the filter cake is replaced and washed 3 times with an equal amount of filtrate pure water, which takes about 40 minutes to obtain a water-containing solid iron hydroxide mixture, and then freeze-dried and dried at 0.1mbar and 5℃ to remove water to obtain high-activity and high-purity iron hydroxide 1.

[0068] Preparation Example 2

[0069] Take polyferric sulfate with an iron content of 23wt% to prepare a polyferric sulfate solution with a concentration of 30wt%, prepare a sodium hydroxide solution according to the molar ratio of iron to hydroxide ion of 1:3.05, add the polyferric sulfate solution dropwise to a 40wt% sodium hydroxide solution, stir to fully form a colloid, and measure the pH to be 7.5. The colloid is placed in a cold trap and quickly frozen to -20℃ for 5 hours, then heated to 10℃ and stirred for 30 minutes, filtered at a pressure of 0.3MPa, and the filter cake is replaced and washed 3 times with an equal amount of filtrate pure water, which takes about 40 minutes to obtain a water-containing solid iron hydroxide mixture, and then freeze-dried and dried at -20℃ under 0.35mbar to remove water to obtain high-activity and high-purity iron hydroxide 2.

[0070] Preparation Example 3

[0071] Take polyferric sulfate with an iron content of 21wt% to prepare a polyferric sulfate solution with a concentration of 20wt%, prepare a sodium hydroxide solution according to the molar ratio of iron to hydroxide ion of 1:3.02, add the polyferric sulfate solution dropwise to a 40wt% sodium hydroxide solution, stir to fully form a colloid, and measure the pH to be 7.3. The colloid is placed in a cold trap and quickly frozen to -30°C for 3 hours, then heated to 30°C and stirred for 20 minutes, filtered at a pressure of 0.2MPa, and the filter cake is replaced and washed 3 times with an equal amount of filtrate pure water, which takes about 40 minutes to obtain a water-containing solid iron hydroxide mixture, and then freeze-dried and dried at -5°C under 0.2mbar to remove water to obtain high-activity and high-purity iron hydroxide. Example 1

[0072] 1) adding the prepared and purified p-toluenesulfonic acid monohydrate solid and the high-purity active ferric hydroxide solid obtained in Preparation Example 1 in a molar ratio of 3:1 into a closed oscillating reaction shaker, and mixing and oscillating at a constant temperature of 105° C. for 24 hours;

[0073] 2) Add 3 times the amount of pure water to the ferric p-toluenesulfonate and unreacted impurities, stir at 65°C for 60 minutes to dissolve, and filter after reaching room temperature. The filtrate is the ferric p-toluenesulfonate aqueous solution;

[0074] 3) The filtrate of the aqueous solution of ferric p-toluenesulfonate is decompressed by 0.085 MPa and heated to 75°C, and the aqueous solution of ferric p-toluenesulfonate is concentrated until a large amount of p-toluenesulfonic acid flaky crystals are precipitated, and the filter cake is high-purity hydrous ferric p-toluenesulfonate flaky crystals;

[0075] 4) The ferric p-toluenesulfonate flake crystals were decompressed to 0.085 MPa and dried at a constant temperature of 165°C for 4 hours to obtain a solid product. Example 2

[0076] 1) adding the prepared and purified p-toluenesulfonic acid monohydrate solid and the high-purity active ferric hydroxide solid obtained in Preparation Example 2 in a molar ratio of 3:1 into a closed oscillating reaction shaker, and mixing and oscillating at a constant temperature of 120° C. for 16 hours;

[0077] 2) Add 2 times amount of pure water to the ferric p-toluenesulfonate and unreacted impurities, stir at 95°C for 30 minutes to dissolve, and filter after reaching room temperature. The filtrate is the ferric p-toluenesulfonate aqueous solution;

[0078] 3) The filtrate of the aqueous solution of ferric p-toluenesulfonate is depressurized to 0.1 MPa and heated to 95°C, and the aqueous solution of ferric p-toluenesulfonate is concentrated until a large amount of p-toluenesulfonic acid flaky crystals are precipitated, and the filter cake is high-purity hydrous ferric p-toluenesulfonate flaky crystals;

[0079] 4) The ferric p-toluenesulfonate flake crystals were decompressed to 0.1 MPa and dried at a constant temperature of 195°C for 10 hours to obtain a solid product. Example 3

[0080] 1) adding the prepared and purified p-toluenesulfonic acid monohydrate and the high-purity active ferric hydroxide solid obtained in Preparation Example 3 in a molar ratio of 3:1 into a closed oscillating reaction shaker and mixing and oscillating at a constant temperature of 110° C. for 20 hours;

[0081] 2) Add 3 times the amount of pure water to the ferric p-toluenesulfonate and unreacted impurities, stir at 90°C for 50 minutes to dissolve, and filter after reaching room temperature. The filtrate is the ferric p-toluenesulfonate aqueous solution;

[0082] 3) The filtrate of the aqueous solution of ferric p-toluenesulfonate is decompressed by 0.09 MPa and heated to 90°C, and the aqueous solution of ferric p-toluenesulfonate is concentrated until a large amount of p-toluenesulfonic acid flaky crystals are precipitated, and the filter cake is high-purity hydrous ferric p-toluenesulfonate flaky crystals;

[0083] 4) The ferric p-toluenesulfonate flake crystals were decompressed to 0.09 MPa and dried at a constant temperature of 180°C for 6 hours to obtain a solid finished product.

[0084] Comparative Example 1

[0085] Prepare the same polyferric sulfate and sodium hydroxide solution as in Preparation Example 1 respectively, add the sodium hydroxide solution dropwise to the polyferric sulfate solution, and after the addition is completed, the pH value of the stirred mixed solution is 6.5, the colloid viscosity is too large, it is impossible to stir, the reaction is insufficient, it is impossible to pressurize or filter under reduced pressure, and it is impossible to separate sodium hydroxide, sodium sulfate and water. The mixed solution is layered after standing for 7 days, the upper colorless liquid is poured out, and the lower layer is filtered under reduced pressure of 0.1MPa to obtain a mixed solid. A single equal amount of filtrate pure water replacement and reduced pressure filtration still takes 4 days, and a mixed solid is finally obtained after 2 pure water replacements.

[0086] Comparative Example 2

[0087] The preparation process is the same as that of Preparation Example 1, except that the colloid is placed in a cold trap and quickly frozen to -10°C for 5 hours, then heated to 10°C and stirred for 30 minutes.

[0088] Comparative Example 3

[0089] The preparation process is the same as that of Preparation Example 1, except that the filter cake after filtration is not replaced and washed with pure water.

[0090] Comparative Example 4

[0091] The preparation process is the same as that of Preparation Example 1, except that the aqueous ferric hydroxide solid mixture is dried at 5°C and 100 mba.

[0092] Comparative Example 5

[0093] The preparation process is the same as that of Preparation Example 3, except that the aqueous ferric hydroxide solid mixture is dried at 110° C. and normal pressure.

[0094] Comparative Example 6

[0095] The preparation process is the same as that of Example 1, except that freshly prepared (iron sulfate reacts with sodium hydroxide) or commercially available iron hydroxide crystals are used. After the reaction is completed, the solution is brown-yellow turbid, and a large amount of p-toluenesulfonic acid is present. Iron hydroxide does not participate in the reaction. After standing and stratifying, the upper brown-red liquid is poured out and filtered.

[0096] Comparative Example 7

[0097] The preparation process is the same as that of Example 1, except that p-toluenesulfonic acid which has not been purified by barium hydroxide is used for the reaction.

[0098] Comparative Example 8

[0099] The prepared and purified p-toluenesulfonic acid monohydrate and the high-activity high-purity ferric hydroxide prepared in Preparation Example 1 were mixed in a molar ratio of 3:1 and added to a closed oscillating reactor, and oscillated at a constant temperature of 105°C for 24 hours. After the reaction was completed, it was cooled to room temperature, ethanol was added, and the temperature was raised to 50 degrees Celsius for 30 minutes to stir and dissolve. The solution was reddish brown, and the bottom was brownish yellow and insoluble, and a brownish yellow solid was obtained by filtration.

[0100] Experimental Example 1

[0101] The colloid obtained in Comparative Example 1 was dehydrated and then subjected to XRD and SEM analysis. The colloid obtained in Preparation Examples 1 to 3 before quenching was dehydrated and then subjected to XRD analysis. The iron hydroxide finally obtained in Preparation Examples 1 to 3 was also subjected to XRD and SEM analysis. The XRD results are as follows: Figure 2 As shown, curve 3 represents the analysis results of comparative example 1, and curve 1 represents the analysis results of the final products obtained in preparation examples 1 to 3 (the same Figure 1), Curve 2 represents the analysis results of the colloidal products obtained in Preparation Examples 1 to 3 before quenching. Figure 3 In the SEM images shown, A represents the analysis results of Examples 1 to 3, and B represents the analysis results of Comparative Example 1. A is obviously amorphous, while B is a typical crystalline form. Correspondingly, Figure 2 The XRD curve 3 shows obvious diffraction peaks, which is fixed crystalline iron hydroxide, causing the iron hydroxide to lose activity. Curve 2 reflects amorphous iron hydroxide, but there are many diffraction peaks in this curve, indicating that the substance has many diffraction products with high impurity content. The sulfate ion content in comparative example 1 is >10000ppm by turbidimetry, and the sodium ion content is 11315ppm by flame photometer. The high impurity content affects the diffraction peaks; there is no obvious diffraction peak in curve 1, which is amorphous.

[0102] The ferric hydroxide products obtained in Preparation Examples 1-3 and Comparative Examples 1-3 were analyzed for purity, yield and other indicators. The ferric hydroxide content was detected and calculated according to GB1886.25-2016. The sodium ion content of the samples was detected by a flame photometer after de-ironification, and the ferric hydroxide yield (calculated as polyferric sulfate) was shown in Table 1.

[0103] Table 1:

[0104] sample Iron hydroxide content wt% Water content wt% Sodium content ppm Iron hydroxide yield% Preparation Example 1 98.45 1.53 15 99.88 Preparation Example 2 98.52 1.46 13 99.90 Preparation Example 3 98.57 1.41 10 99.89 Comparative Example 1 28.80 71.18 >10000 -- Comparative Example 2 70.18 27.4 >10000 99.53 Comparative Example 3 96.21 1.58 4690 99.65

[0105] It is not difficult to see from Table 1 that the purity (excluding water) content of the iron hydroxide solid obtained in Preparation Examples 1-3 reaches 99.98wt%, and the sodium ion content is less than 50ppm, which is relatively ideal and is an ideal choice for the subsequent preparation of ferric p-toluenesulfonate. In comparison, when the reverse addition is added in Comparative Example 1, the iron hydroxide colloid with suitable viscosity cannot be normally generated. The reason is that when the alkali solution is added dropwise to the polyferric sulfate, the polyferric sulfate is relatively excessive, forming self-adsorption, resulting in excessive viscosity and inability to perform subsequent operations, resulting in an unsatisfactory product. Comparative Example 2 is frozen at -10°C, resulting in a large amount of impurities that cannot be desorbed, resulting in a decrease in its purity. In addition, it is not freeze-dried and dried, and the moisture content is high; Comparative Example 3 does not wash the filter cake with pure water, resulting in a large amount of sodium sulfate adsorbed on the surface of the iron hydroxide not being removed, affecting the purity.

[0106] By performing SEM analysis on the products obtained in Examples 4-5, it was found that the drying process caused changes in the solid morphology, corresponding to the following: Figure 4 As shown in A and B, it can be seen that both SEM images show a crystalline form. Since the comparative example 4 takes a long time to dry (more than 100 times the normal freeze-drying time), it is transformed into a crystalline form. The conventional drying method of comparative example 5 will also transform the amorphous form into a crystalline form.

[0107] Experimental Example 2

[0108] The products of ferric p-toluenesulfonate obtained in Examples 1-3 and Comparative Examples 6-7 were analyzed for purity and yield, and the content of ferric p-toluenesulfonate was detected and calculated. The sodium ion content of the samples was detected by a flame photometer after de-ironification. The results are shown in Table 2.

[0109] Table 2:

[0110] sample Iron p-toluenesulfonate content wt% Water content wt% Sulfate content ppm Yield of ferric p-toluenesulfonate % Example 1 99.92 0.07 41 99.88 Example 2 99.92 0.08 40 99.90 Example 3 99.91 0.09 39 99.89 Comparative Example 6 18.50 82.45 >10000 15.75 Comparative Example 7 97.56 0.10 >10000 95.53

[0111] It is not difficult to see from Table 2 that the content and yield of the iron p-toluenesulfonate obtained in Examples 1-3 are relatively ideal. In comparison, Comparative Example 6 uses existing or commercially available iron hydroxide crystals to participate in the reaction, which has a high impurity content and low activity, and the purity and yield of the product are greatly reduced. The reason is that Examples 1-3 use amorphous iron hydroxide, which is in a non-crystalline state and has a strong reaction activity; Comparative Example 7 uses unpurified p-toluenesulfonic acid, which contains sulfate impurities that affect the quality of the product.

[0112] Experimental Example 3

[0113] The obtained ferric p-toluenesulfonate solids of Examples 1-3 and Comparative Example 8 were cooled to room temperature and then dissolved in ethanol to prepare ferric p-toluenesulfonate-ethanol solutions with a mass content of 50%. The ratio of iron to sulfur was analyzed, as shown in Table 3.

[0114] Table 3:

[0115] sample Iron: Sulfur Comparative Example 8 1:3.42 Example 1 1:3.02 Example 2 1:2.99 Example 3 1:3.01

[0116] The molecular formula of ferric p-toluenesulfonate is C 21 H 21 FeO9S3, it is not difficult to see from Table 1 that the ferric p-toluenesulfonate obtained in Examples 1 to 3 is very close to 1:3, which further illustrates that the prepared ferric p-toluenesulfonate has a high purity. In Comparative Example 8, no crystallization and impurity removal was performed, resulting in the mixing of sulfate impurities, which affected the purity.

[0117] The above-mentioned iron p-toluenesulfonate-ethanol solution with a solid content of 50% was mixed with commercially available EDOT and prepolymerized at room temperature for 2 hours. Then, the capacitor aluminum foil was impregnated, cured at 110 degrees Celsius, and dried to prepare a specific solid aluminum capacitor cathode material. The material was tested for performance, and the results are shown in Table 4.

[0118] Table 4:

[0119] sample Cathode material conductivity (S / cm) Solid capacitor ESR (mΩ) Sulfonic acid content ppm Sulfate content ppm Comparative Example 8 630 7.52 >10000 >10000 Example 1 1275 3.45 37 44 Example 2 1269 3.46 36 42 Example 3 1274 3.45 39 38 Commercially available products 830 4.38 3610 580

[0120] It is not difficult to see from Table 4 that the solid aluminum capacitor cathode material obtained by reacting the high-purity iron p-toluenesulfonate obtained in Examples 1-3 with EDOT has excellent performance. Compared with Examples 1-3, Comparative Example 8 and the commercially available products have higher impurity content in the finished products. After being prepared into a conductive polymer cathode material, the impurities participate in the mixing, resulting in the cathode material being mixed with impurities such as p-toluenesulfonic acid and sodium sulfate. p-Toluenesulfonic acid is a protonic acid. When it exists in excess, it has the effect of inhibiting and slowing down the polymerization speed and depth during the EDOT polymerization process, thereby reducing the conductivity and the solid capacitor equivalent series resistance (ESR) is too large after application. When the conductivity is low and the equivalent series resistance is too large, the solid capacitor's heat generation, leakage current, DC isolation, life and other performances in the circuit board are affected.

[0121] In summary, the preparation of high-purity and high-activity iron hydroxide and its reaction with high-purity p-toluenesulfonic acid containing monocrystalline water to prepare ultra-clean high-purity iron p-toluenesulfonate, which is applied to solid aluminum capacitors, has obvious advantages over existing technologies in improving the performance parameters of terminal products.

[0122] Finally, a few points should be explained. Although the present invention has been described in detail above with general descriptions and specific embodiments, on the basis of the present invention, the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing high-activity and high-purity ferric hydroxide, It is characterized in that The steps include: S1. The polyferric sulfate solution is slowly added dropwise to the alkaline solution to a pH value of 7.0 to 7.5; the iron content of the polyferric sulfate is 19-23wt%; S2. Freeze the system obtained in step S1 at -20~-50°C for 1~5h, then heat to 10~38°C and stir for 5~30min; S3. The system obtained in step S2 is filtered, washed with water, and then freeze-dried to obtain high-activity and high-purity ferric hydroxide; the freeze-drying conditions are 0.1~0.35mbar and -20~5°C.

2. The method for preparing ferric hydroxide according to claim 1, It is characterized in that The step S3 is filtering under a pressure of 0.1-0.3 MPa.

3. The ferric hydroxide obtained by the preparation method according to any one of claims 1 to 2, It is characterized in that The iron hydroxide has an amorphous state.

4. A method for preparing ferric p-toluenesulfonate, It is characterized in that Add p-toluenesulfonic acid monohydrate and solid ferric hydroxide in a molar ratio of 3:1 into a closed shaking reaction shaker at 105-120° C. and mix and shake for 16-24 hours, filter, and crystallize the filtrate to obtain ferric p-toluenesulfonate; the ferric hydroxide is the ferric hydroxide according to claim 3.

5. The preparation method according to claim 4, It is characterized in that After the oscillation reaction, add 2 to 3 times the amount of pure water to the system obtained, stir at 65 to 95°C for 30 to 60 minutes to dissolve, and then filter.

6. The preparation method according to claim 4, It is characterized in that The p-toluenesulfonic acid monohydrate is prepared by mixing industrial p-toluenesulfonic acid with 1-3% by mass of barium hydroxide at 40-75° C., stirring for 2-5 hours, adding lignin, filtering, and crystallizing to obtain the p-toluenesulfonic acid monohydrate.

7. The preparation method according to claim 4, It is characterized in that The filtrate is heated to 75-95° C. under a negative pressure of 0.085-0.1 MPa for concentration and crystallization.

8. Use of the iron p-toluenesulfonate obtained by the preparation method according to any one of claims 4 to 7 in the preparation of cathode materials for solid-state aluminum capacitors.