A hydrophobic glass substrate and its preparation method and application
The method of forming a columnar structure through laser treatment and soaking it in a specific silane solution solves the problems of complicated preparation and poor hydrophobicity of hydrophobic glass in the existing technology, and achieves efficient hydrophobicity and self-cleaning antifouling properties, which is suitable for automobiles and Architectural glass.
Patent Information
- Application Number
- CN202210806272.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-08
AI Technical Summary
The preparation process of hydrophobic glass in the prior art is complicated and has poor hydrophobicity, which cannot effectively prevent contamination by dust and other pollutants, affecting clear vision and personal safety.
A glass substrate with a columnar structure is formed by laser treatment, and then immersed in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane for drying to form a superhydrophobic surface.
A hydrophobic glass substrate with a contact angle greater than 150° was obtained, which has self-cleaning and antifouling properties and can effectively prevent the adhesion of dust and particulate pollutants.
Smart Images

Figure CN115215554B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass surface modification, and in particular to a hydrophobic glass substrate and a preparation method and application thereof. Background Art
[0002] Glass is a widely used material in daily life and industrial production, such as architectural glass, automotive glass, etc. When glass is used outdoors, it is often contaminated by pollutants such as dust, which brings inconvenience to people's work and life, and poses certain hidden dangers to personal safety.
[0003] After millions of years of evolution, a large number of organisms in nature have formed natural and reasonable superhydrophobic structures. Typical biological superhydrophobic structures include lotus leaves, cicada wings and rice leaves. The microstructures and low surface energy chemical composition of these biological surfaces give them excellent superhydrophobicity and self-cleaning and antifouling properties.
[0004] Therefore, in terms of engineering material design and manufacturing, it is of great significance to endow glass with superhydrophobicity and self-cleaning and antifouling properties.
[0005] In order to obtain hydrophobic glass, the prior art generally involves spraying a hydrophobic coating on the glass surface, or evaporating a layer of hydrophobic coating liquid.
[0006] CN1778749A discloses a glass hydrophobic coating liquid, which is composed of a long-chain alkyl silane coupling agent, an alkyl silicate, an alcohol, an inorganic acid catalyst and deionized water or distilled water. The glass hydrophobic coating liquid can form a transparent hydrophobic film on the surface of automobile glass. Water droplets can form water beads on the glass surface, and the contact angle can be as high as 110°C. Water beads can roll off automatically without leaving any traces, thereby solving the problem of unclear vision.
[0007] However, the coating preparation process obtained by the aforementioned method is complicated, and the obtained coating is easy to fall off and has the defect of poor hydrophobicity. Summary of the invention
[0008] The purpose of the present invention is to overcome the defects of the hydrophobic glass in the prior art, such as the complicated preparation process and poor hydrophobicity.
[0009] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a hydrophobic glass substrate, the method comprising:
[0010] (1) laser processing the surface of a glass substrate to obtain a glass substrate I having a plurality of columnar structures; the aspect ratio of the columnar structures is 1:1-3, and the spacing between adjacent columnar structures is 80 μm-120 μm;
[0011] (2) immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and subjecting the glass substrate II to a first drying treatment; in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.1-3% by volume.
[0012] Preferably, in step (1), the laser treatment is performed in the presence of ultraviolet light.
[0013] Preferably, in step (1), the laser processing conditions include at least: a pulse width of 100-200ns, a pulse repetition frequency of 10-30kHz, a laser power of 40-60W, an effective spot diameter after focusing of about 30-50μm, and a laser scanning rate of 400-600mm / s.
[0014] Preferably, in step (1), the aspect ratio of the columnar structure is 1:1.2-2.
[0015] Preferably, in step (2), in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.5-2% by volume.
[0016] Preferably, in step (2), the soaking conditions at least include: a temperature of 20-40° C. and a time of 12-24 h.
[0017] Preferably, in step (2), the method further comprises: before immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane, first subjecting the glass substrate I to a second cleaning treatment and a second drying treatment in sequence.
[0018] Preferably, in step (2), the conditions of the first drying treatment at least include: a temperature of 20-40° C. and a time of 6-12 h.
[0019] Preferably, in step (2), the method further comprises: before performing the first drying treatment, performing a first cleaning on the glass substrate II.
[0020] The second aspect of the present invention provides a hydrophobic glass substrate prepared by the method described in the first aspect.
[0021] The third aspect of the present invention provides use of the hydrophobic glass substrate described in the second aspect in automotive glass and architectural glass.
[0022] The glass substrate prepared by the method provided by the present invention has enhanced hydrophobicity, a contact angle greater than 150°, and can also achieve self-cleaning and anti-fouling properties on the glass surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the contact angle of the hydrophobic glass substrate prepared in Example 1 of the present invention;
[0024] Figure 2 Schematic diagram of contact angle of glass substrate in control group;
[0025] Figure 3 It is a schematic diagram of the cleaning and antifouling process of the hydrophobic glass substrate prepared in Example 1 of the present invention.
[0026] Description of Reference Numerals
[0027] 1. Water droplets 2. Hydrophobic glass substrate
[0028] 3. Glass substrate of control group 4. Dust and particle contaminants DETAILED DESCRIPTION
[0029] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0030] In the present invention, unless otherwise specified, the room temperature or normal temperature refers to 25±2°C.
[0031] In the present invention, the aspect ratio of the columnar structure refers to “the ratio of the height of the columnar structure to the diameter of the columnar structure”.
[0032] As mentioned above, the first aspect of the present invention provides a method for preparing a hydrophobic glass substrate, the method comprising:
[0033] (1) laser processing the surface of a glass substrate to obtain a glass substrate I having a plurality of columnar structures; the aspect ratio of the columnar structures is 1:1-3, and the spacing between adjacent columnar structures is 80 μm-120 μm;
[0034] (2) immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and subjecting the glass substrate II to a first drying treatment; in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.1-3% by volume.
[0035] The inventors of the present invention discovered during the research process that a super-hydrophobic surface can be formed on the glass surface by using a micro-nano hierarchical structure formed by laser processing and sputtering, in combination with an ethanol solution containing a specific concentration of 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane. The obtained contact angle of the glass substrate surface is greater than 150°, achieving a super-hydrophobic state.
[0036] The present invention has no special requirements on the size of the glass substrate, and glass substrates of different sizes can be designed according to demand. For example, the glass substrate can be (1-20) cm×(1-20) cm×(0.1-0.5) cm.
[0037] Preferably, in step (1), the laser treatment is performed in the presence of ultraviolet light.
[0038] According to a particularly preferred specific embodiment, in step (1), the conditions of the laser processing include at least: a pulse width of 100-200ns, a pulse repetition frequency of 10-30kHz, a laser power of 40-60W, an effective spot diameter after focusing of about 30-50μm, and a laser scanning rate of 400-600mm / s.
[0039] According to a particularly preferred embodiment of the present invention, in step (1), the height-to-diameter ratio of the columnar structure is 1:1.2-2. The inventors have found that by adopting the specific embodiment of this preferred case, a glass substrate with better hydrophobic properties can be obtained.
[0040] According to a particularly preferred embodiment of the present invention, in step (2), in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.5-2% by volume. The inventors have found that in this preferred embodiment, a glass substrate with better hydrophobic properties can be prepared.
[0041] According to a particularly preferred embodiment of the present invention, in step (2), relative to 3 cm 2 The glass substrate I, the amount of the ethanol solution is 50-100mL.
[0042] Preferably, in step (2), the soaking conditions at least include: a temperature of 20-40° C. and a time of 12-24 h.
[0043] Preferably, in step (2), the method further comprises: before immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane, first subjecting the glass substrate I to a second cleaning treatment and a second drying treatment in sequence.
[0044] Preferably, in step (2), the solvent for the second cleaning is ethanol, and the second cleaning is performed under ultrasonic conditions.
[0045] According to a particularly preferred embodiment, in step (2), the second cleaning conditions at least include: ultrasonic power of 100-200W, temperature of 20-30°C.
[0046] According to a particularly preferred embodiment, in step (2), the conditions of the second drying treatment at least include: a temperature of 20-40° C. and a time of 0.2-1 h.
[0047] Preferably, in step (2), the conditions of the first drying treatment at least include: a temperature of 20-40° C. and a time of 6-12 h.
[0048] According to a particularly preferred embodiment of the present invention, in step (2), the method further comprises: before performing the first drying treatment, first cleaning the glass substrate II.
[0049] Preferably, in step (2), the solvent for the first cleaning is ethanol, and the number of times of the first cleaning is 1-5 times.
[0050] As mentioned above, the second aspect of the present invention provides a hydrophobic glass substrate prepared by the method described in the first aspect.
[0051] As mentioned above, the third aspect of the present invention provides the use of the hydrophobic glass substrate described in the second aspect in automotive glass and architectural glass.
[0052] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all the raw materials and instruments used are commercially available.
[0053] 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane: purchased from Aladdin Reagent Co., Ltd.;
[0054] In the following examples, laser treatment was performed in an ultraviolet laser instrument (model UV-50, purchased from Changchun New Industries Optoelectronics Technology Co., Ltd.).
[0055] Example 1
[0056] This embodiment provides a method for preparing a hydrophobic glass substrate, the method comprising:
[0057] (1) treating the surface of a glass substrate with ultraviolet laser to obtain a glass substrate I having a plurality of columnar structures;
[0058] The diameter of the columnar structure is 50 μm, the height is 60 μm, and the spacing between adjacent columnar structures is 100 μm.
[0059] The conditions of UV laser treatment are: laser wavelength of 350nm, pulse width of 150ns, pulse repetition frequency of 20kHz, laser power of 50W, effective spot diameter after focusing of about 40μm, laser scanning rate of 500mm / s;
[0060] (2) The glass substrate I was ultrasonically cleaned in ethanol (ultrasonic power of 150 W, temperature of 25° C.), dried at room temperature for 0.5 h, and then immersed in an ethanol solution containing 1H, 1H, 2H, 2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and the glass substrate II was rinsed with ethanol for 3 times, and finally subjected to a first drying treatment to obtain a hydrophobic glass substrate S1;
[0061] Wherein, in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 1% by volume, and the amount of the ethanol solution is 200 mL;
[0062] The conditions for the first drying treatment are: room temperature and 8 hours.
[0063] Example 2
[0064] This embodiment provides a method for preparing a hydrophobic glass substrate, the method comprising:
[0065] (1) treating the surface of a glass substrate with ultraviolet laser to obtain a glass substrate I having a plurality of columnar structures;
[0066] The diameter of the columnar structure is 40 μm, the height is 60 μm, and the spacing between adjacent columnar structures is 100 μm.
[0067] The conditions of UV laser treatment are: laser wavelength of 350nm, pulse width of 150ns, pulse repetition frequency of 20kHz, laser power of 50W, effective spot diameter after focusing of about 40μm, laser scanning rate of 500mm / s;
[0068] (2) The glass substrate I was ultrasonically cleaned in ethanol (ultrasonic power of 150 W, temperature of 25° C.), dried at room temperature for 0.5 h, and then immersed in an ethanol solution containing 1H, 1H, 2H, 2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and the glass substrate II was rinsed with ethanol for 3 times, and finally a first drying treatment was performed to obtain a hydrophobic glass substrate S2;
[0069] Wherein, in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 2% by volume, and the amount of the ethanol solution is 200 mL;
[0070] The conditions for the first drying treatment are: room temperature and 8 hours.
[0071] Example 3
[0072] This embodiment provides a method for preparing a hydrophobic glass substrate, the method comprising:
[0073] (1) treating the surface of a glass substrate with ultraviolet laser to obtain a glass substrate I having a plurality of columnar structures;
[0074] The diameter of the columnar structure is 50 μm, the height is 80 μm, and the spacing between adjacent columnar structures is 100 μm.
[0075] The conditions of UV laser treatment are: laser wavelength of 350nm, pulse width of 150ns, pulse repetition frequency of 20kHz, laser power of 50W, effective spot diameter after focusing of about 40μm, laser scanning rate of 500mm / s;
[0076] (2) The glass substrate I was ultrasonically cleaned in ethanol (ultrasonic power of 150 W, temperature of 25° C.), dried at room temperature for 0.5 h, and then immersed in an ethanol solution containing 1H, 1H, 2H, 2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and the glass substrate II was rinsed with ethanol for 3 times, and finally subjected to a first drying treatment to obtain a hydrophobic glass substrate S3;
[0077] Wherein, in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.5% by volume, and the amount of the ethanol solution is 200 mL;
[0078] The conditions for the first drying treatment are: room temperature and 8 hours.
[0079] Example 4
[0080] A hydrophobic glass substrate was prepared according to the method of Example 1, except that in step (1), the height of the columnar structure was 50 μm.
[0081] The remaining steps are the same as those in Example 1 to obtain a hydrophobic glass substrate S5.
[0082] Example 5
[0083] A hydrophobic glass substrate was prepared according to the method of Example 1, except that in step (2), the concentration of 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane in the ethanol solution was 3% by volume, and the amount of the ethanol solution was 200 mL.
[0084] The remaining steps are the same as those in Example 1 to obtain a hydrophobic glass substrate S6.
[0085] Comparative Example 1
[0086] A hydrophobic glass substrate was prepared according to the method of Example 1, except that in step (1), the height of the columnar structure was 30 μm.
[0087] The remaining steps are the same as those in Example 1 to obtain a hydrophobic glass substrate DS1.
[0088] Comparative Example 2
[0089] A hydrophobic glass substrate was prepared according to the method of Example 1, except that in step (2), an equal volume of hexadecyltrimethoxysilane was used to replace 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane.
[0090] The remaining steps are the same as those in Example 1 to obtain a hydrophobic glass substrate DS2.
[0091] Test Case
[0092] The hydrophobic performance of the hydrophobic glass substrates prepared in the examples and comparative examples was tested, and the untreated glass substrate was used as a control group (hereinafter referred to as LS1). The specific test results are shown in Table 1.
[0093] The contact angle test method is as follows: using a DSA25S optical contact angle meter (Germany), selecting distilled water as the test liquid, setting the volume of the distilled water droplet to 5 μL, selecting five different positions on the same sample surface for contact angle measurement, and taking the average value of the measurement results as the contact angle value.
[0094] Table 1
[0095] Example No. Contact angle / ° Example 1 157.5 Example 2 156.1 Example 3 154.7 Example 4 151.2 Example 5 154.1 Comparative Example 1 121.2 Comparative Example 2 117.8 LS1 17.4
[0096] It can be seen from the results in Table 1 that the glass substrate prepared by the method provided by the present invention has enhanced hydrophobicity, a contact angle greater than 150°, and can also achieve self-cleaning and anti-fouling properties on the glass surface.
[0097] The present invention exemplarily provides a schematic diagram of the contact angle of the control glass substrate and the hydrophobic glass substrate prepared in Example 1 of the present invention, and a schematic diagram of the cleaning and antifouling process of the hydrophobic glass substrate prepared in Example 1 of the present invention, respectively. Figure 1 , Figure 2 and Figure 3 .
[0098] in, Figure 1 Schematic diagram of the contact angle of the hydrophobic glass substrate prepared in Example 1 of the present invention, Figure 2 Schematic diagram of contact angle of the glass substrate of the control group, wherein 1 is a water droplet, 2 is the hydrophobic glass substrate prepared in Example 1 of the present invention, and 3 is the glass substrate of the control group.
[0099] from Figure 1 and Figure 2 It can be seen that the hydrophobic glass substrate prepared by the method provided by the present invention has excellent hydrophobic properties, and its contact angle is 157.5°; while the untreated ordinary glass substrate maintains the original hydrophilic state, and the contact angle is 17.4°.
[0100] Figure 3 Schematic diagram of the cleaning and antifouling process of the hydrophobic glass substrate prepared in Example 1 of the present invention, wherein 1 is a water droplet, 2 is the hydrophobic glass substrate prepared in Example 1 of the present invention, and 4 is dust and particulate pollutants.
[0101] from Figure 3 It can be seen that when dust and particle contamination exist on the hydrophobic glass substrate provided by the present invention, when water droplets fall on the surface of the hydrophobic glass substrate, the dust and particle contaminants can be quickly cleaned away. Compared with traditional glass, the hydrophobic glass substrate provided by the present invention also has excellent self-cleaning performance.
[0102] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a hydrophobic glass substrate, characterized in that: The method includes: (1) The surface of a glass substrate is laser treated to obtain a glass substrate I having a plurality of columnar structures; the aspect ratio of the columnar structures is 1:1.2-2, and the spacing between adjacent columnar structures is 80 μm-120 μm; the laser treatment conditions include at least: a pulse width of 100-200 ns, a pulse repetition frequency of 10-30 kHz, a laser power of 40-60 W, an effective spot diameter of 30-50 μm after focusing, and a laser scanning rate of 400-600 mm / s; (2) immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane to obtain a glass substrate II, and subjecting the glass substrate II to a first drying treatment; in the ethanol solution, the concentration of the 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane is 0.5-2% by volume; the immersion conditions at least include: a temperature of 20-40° C. and a time of 12-24 hours; In step (2), the method further includes: before immersing the glass substrate I in an ethanol solution containing 1H,1H,2H,2H-heptadecafluorodecyltriethoxysilane, first subjecting the glass substrate I to a second cleaning treatment and a second drying treatment in sequence.
2. The method according to claim 1, characterized in that In step (1), the laser treatment is performed in the presence of ultraviolet light.
3. The method according to claim 1 or 2, characterized in that: In step (2), the conditions of the first drying treatment include at least: a temperature of 20-40° C. and a time of 6-12 hours.
4. The method according to claim 1 or 2, characterized in that: In step (2), the method further includes: before performing the first drying treatment, first cleaning the glass substrate II.
5. A hydrophobic glass substrate prepared by the method according to any one of claims 1 to 4.
6. Use of the hydrophobic glass substrate according to claim 5 in automobile glass and architectural glass.