Hot melt adhesive film containing anti-scratch coating and preparation method thereof

By coating the hot-melt adhesive film with an anti-scratch coating mixed with nanocomposite resin and HDI, combined with the preparation of a modified EVA adhesive film, the problem that the hot-melt adhesive film cannot be scratch-resistant is solved and a better Protective effect and simple preparation process.

CN115232576BActive Publication Date: 2024-10-29ZHANGJIAJIE GEN Q NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210893041.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-27
Publication Date
2024-10-29
Estimated Expiration
2042-07-27

AI Technical Summary

Technical Problem

The existing hot melt adhesive film cannot achieve the anti-scratch function, and there is a problem of incomplete protection of the product.

Method used

The anti-scratch coating is prepared by mixing nanocomposite resin and HDI, and the coating is coated on the modified EVA film. Combined with the preparation of the modified EVA film, through the modification of nano-silica and the combination of EVA and low density The blending of polyethylene resin improves the adhesiveness and aging resistance of the film.

Benefits of technology

Effective anti-scratch protection of the product is achieved, the service life is improved, the preparation process is simplified, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003768328130000061
    Figure BDA0003768328130000061
Patent Text Reader

Abstract

The present invention relates to the field of hot melt adhesive film materials, and in particular to a hot melt adhesive film containing an anti-scratch coating, comprising an anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano-composite resin with HDI, and the nano-composite resin is composed of the following raw materials in parts by weight: 70-90 parts of hydroxy acrylate, 30-50 parts of nano-silicon dioxide, and 10-20 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 60-85 parts of EVA; 25-40 parts of low-density polyethylene resin; 5-8 parts of a coupling agent; and 1-4 parts of an antioxidant. The present invention provides a hot melt adhesive film containing an anti-scratch coating with good protective effect. The present invention also provides a method for preparing a hot melt adhesive film containing an anti-scratch coating, which has a simpler process, saves preparation costs, simplifies the preparation process, and has the characteristics of strong practicality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hot melt adhesive film materials, in particular to a hot melt adhesive film containing an anti-scratch coating and a preparation method thereof. Background Art

[0002] Hot melt adhesive film is a film product with or without release paper, which can be conveniently operated continuously or intermittently. It can be widely used for bonding various fabrics, paper, polymer materials and metals.

[0003] The current hot melt adhesive film cannot achieve the anti-scratch function and has the problem of incomplete protection of the product. For this reason, we propose a hot melt adhesive film containing an anti-scratch coating. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a hot melt adhesive film with a scratch-resistant coating and good protective effect.

[0005] The present invention also provides a method for preparing a hot melt adhesive film containing an anti-scratch coating, which has a simpler process, saves preparation costs, simplifies the preparation process, and has the characteristics of strong practicality.

[0006] The present invention adopts the following technical solution:

[0007] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano composite resin with HDI, the nano composite resin is composed of the following raw materials in parts by weight: 70-90 parts of hydroxy acrylate, 30-50 parts of nano silicon dioxide, and 10-20 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 60-85 parts of EVA; 25-40 parts of a low-density polyethylene resin; 5-8 parts of a coupling agent; and 1-4 parts of an antioxidant.

[0008] A further improvement to the above technical solution is that the hydroxy value of the hydroxy acrylate is 110-135 mgKOH / g and the solid content is 40-65%.

[0009] A further improvement to the above technical solution is that the specific surface area of ​​the nano-silicon dioxide is 400-600m 2 / g, and the primary particle size is 12-18nm.

[0010] A further improvement to the above technical solution is that the modifier is one of a silane coupling agent, a titanate coupling agent, and a hyperdispersant, preferably γ-methacryloxypropyltrimethoxysilane.

[0011] A further improvement to the above technical solution is that the preparation method of the nanocomposite resin comprises the following steps:

[0012] S1. Preparation of modified nano-silicon dioxide: pre-dispersing nano-silicon dioxide in a toluene solution containing a modifier, stirring and reacting at 85-100° C. for 10-15 hours, then centrifuging and washing with an ethanol solution, centrifuging for 4-5 times, and finally drying at 65-80° C. for 12-20 hours to obtain modified nano-silicon dioxide;

[0013] S2. Preparation of nano-composite resin: The nano-composite resin is prepared by mixing the modified nano-silica with hydroxy acrylate by high-speed shearing or by ultrasonic mixing with a mixed monomer solution and then polymerizing.

[0014] A further improvement to the above technical solution is that the EVA is one or more of EVA250, EVA550, and EVA650.

[0015] A further improvement to the above technical solution is that the coupling agent is one of a silane coupling agent and a titanate coupling agent.

[0016] A further improvement to the above technical solution is that the antioxidant is one of a hindered phenol antioxidant, a hindered amine antioxidant or a phosphite antioxidant.

[0017] A further improvement to the above technical solution is that the method for preparing the modified EVA film comprises the following steps:

[0018] S1. Add the weighed EVA and low-density polyethylene resin into a mixer, start stirring, then add antioxidant and coupling agent into the mixer in sequence, stir and mix for 10-20 minutes, stop stirring after stirring evenly, and obtain an EVA modified mixture;

[0019] S2. Adding the EVA modified mixture into the pre-heated casting machine hopper to obtain a modified EVA film, the casting temperature is 150-180°C.

[0020] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0021] The beneficial effects of the present invention are:

[0022] The invention prepares a modified EVA film by blending and modifying EVA and low-density polyethylene resin. The modified EVA film has excellent bonding performance, heat resistance and aging resistance, and meets the requirements of composite bonding of existing products. An anti-scratch coating is provided, and the surface of nano-silicon dioxide is modified by a modifier, so that the invention has anti-scratch performance, good protection effect, and further improves the service life. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0024] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano composite resin with HDI, the nano composite resin is composed of the following raw materials in parts by weight: 70-90 parts of hydroxy acrylate, 30-50 parts of nano silicon dioxide, and 10-20 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 60-85 parts of EVA; 25-40 parts of a low-density polyethylene resin; 5-8 parts of a coupling agent; and 1-4 parts of an antioxidant.

[0025] Furthermore, the hydroxy value of the hydroxy acrylate is 110-135 mgKOH / g, and the solid content thereof is 40-65%.

[0026] Furthermore, the specific surface area of ​​the nano-silicon dioxide is 400-600m 2 / g, and the primary particle size is 12-18nm.

[0027] Furthermore, the modifier is one of a silane coupling agent, a titanate coupling agent, and a hyperdispersant, preferably γ-methacryloxypropyltrimethoxysilane.

[0028] Furthermore, the preparation method of the nanocomposite resin comprises the following steps:

[0029] S1. Preparation of modified nano-silicon dioxide: pre-dispersing nano-silicon dioxide in a toluene solution containing a modifier, stirring and reacting at 85-100° C. for 10-15 hours, then centrifuging and washing with an ethanol solution, centrifuging for 4-5 times, and finally drying at 65-80° C. for 12-20 hours to obtain modified nano-silicon dioxide;

[0030] S2. Preparation of nano-composite resin: The nano-composite resin is prepared by mixing the modified nano-silica with hydroxy acrylate by high-speed shearing or by ultrasonic mixing with a mixed monomer solution and then polymerizing.

[0031] Furthermore, the EVA is one or more of EVA250, EVA550, and EVA650.

[0032] Furthermore, the coupling agent is one of a silane coupling agent and a titanate coupling agent.

[0033] Furthermore, the antioxidant is one of a hindered phenol antioxidant, a hindered amine antioxidant or a phosphite antioxidant.

[0034] Furthermore, the preparation method of the modified EVA film comprises the following steps:

[0035] S1. Add the weighed EVA and low-density polyethylene resin into a mixer, start stirring, then add antioxidant and coupling agent into the mixer in sequence, stir and mix for 10-20 minutes, stop stirring after stirring evenly, and obtain an EVA modified mixture;

[0036] S2. Adding the EVA modified mixture into the pre-heated casting machine hopper to obtain a modified EVA film, the casting temperature is 150-180°C.

[0037] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0038] Example 1

[0039] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano-composite resin with HDI, the nano-composite resin is composed of the following raw materials in parts by weight: 70 parts of hydroxy acrylate, 30 parts of nano-silicon dioxide, and 10 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 60 parts of EVA; 25 parts of a low-density polyethylene resin; 5 parts of a coupling agent; and 1 part of an antioxidant.

[0040] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0041] Example 2

[0042] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano composite resin with HDI, the nano composite resin is composed of the following raw materials in parts by weight: 80 parts of hydroxy acrylate, 40 parts of nano silicon dioxide, and 15 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 70 parts of EVA; 30 parts of a low-density polyethylene resin; 5 parts of a coupling agent; and 2 parts of an antioxidant.

[0043] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0044] Example 1

[0045] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano composite resin with HDI, the nano composite resin is composed of the following raw materials in parts by weight: 90 parts of hydroxy acrylate, 50 parts of nano silicon dioxide, and 20 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 85 parts of EVA; 40 parts of a low-density polyethylene resin; 8 parts of a coupling agent; and 4 parts of an antioxidant.

[0046] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0047] Comparative Example 1

[0048] A hot melt adhesive film containing an anti-scratch coating comprises the anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano-composite resin with HDI, the nano-composite resin is composed of the following raw materials in parts by weight: 70 parts of nano-silicon dioxide; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 60 parts of EVA; 5 parts of coupling agent; and 1 part of antioxidant.

[0049] A method for preparing a hot melt adhesive film containing an anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of a modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating.

[0050] The hot melt adhesive films containing anti-scratch coatings of Examples 1-3 and Comparative Example 1 were subjected to performance tests respectively, wherein the impact strength test method is as follows: the film to be tested is cut into a specification of 5 cm×2 cm, fixed on a plane, and placed horizontally. A steel ball weighing 32±2 g is selected and dropped vertically at a height of 30 cm. Three points on the diagonal of the film are selected for testing. If the film is not broken after the impact test, the test result is judged to be qualified, otherwise it is unqualified.

[0051] The scratch test is used to detect the anti-scratch performance of the film. The scratch test method is as follows: 1) Fix the film to be tested so that the film coincides with the center of the pendulum of the friction tester; 2) Stick 0000# steel wool to the center of the die, with a total load of 200g and a friction area of ​​2cm×2cm; 3) Start the friction tester, with a friction speed of 30 times / minute and 50 reciprocating frictions; 4) Wash the film that has undergone the above friction test and dry it with cotton paper or air dry it, and observe the surface of the sample after the test. If there are no scratches or scratches on the surface, the test result is judged to be qualified, otherwise it is unqualified. The performance indicators are shown in Table 1.

[0052] Table 1

[0053]

[0054] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made according to the application scope of the present invention are within the scope of the patent of the present invention.

Claims

1. A hot melt adhesive film containing an anti-scratch coating, characterized in that: The invention comprises an anti-scratch coating and an adhesive film layer arranged below the anti-scratch coating; the anti-scratch coating is obtained by mixing a nano-composite resin with HDI, and the nano-composite resin is composed of the following raw materials in parts by weight: 90 parts of hydroxy acrylate, 50 parts of nano-silicon dioxide, and 20 parts of a modifier; the adhesive film layer is a modified EVA adhesive film, and the modified EVA adhesive film is composed of the following raw materials in parts by weight: 85 parts of EVA; 40 parts of a low-density polyethylene resin; 8 parts of a coupling agent; and 4 parts of an antioxidant; The modifier is one of a silane coupling agent, a titanate coupling agent, and a hyperdispersant; The preparation method of the nanocomposite resin comprises the following steps: S1. Preparation of modified nano-silicon dioxide: pre-dispersing nano-silicon dioxide in a toluene solution containing a modifier, stirring and reacting at 85-100° C. for 10-15 hours, then centrifuging and washing with an ethanol solution, centrifuging for 4-5 times, and finally drying at 65-80° C. for 12-20 hours to obtain modified nano-silicon dioxide; S2. Preparation of nanocomposite resin: preparing the nanocomposite resin by mixing the modified nano-silica with hydroxy acrylate by high-speed shearing or ultrasonic mixing with a mixed monomer solution and then polymerizing; The preparation method of the modified EVA film comprises the following steps: S1. Add the weighed EVA and low-density polyethylene resin into a mixer, start stirring, then add antioxidant and coupling agent into the mixer in sequence, stir and mix for 10-20 minutes, stop stirring after stirring evenly, and obtain an EVA modified mixture; S2, adding the EVA modified mixture into the pre-heated casting machine hopper to obtain a modified EVA film, the casting temperature is 150-180°C; The method for preparing the hot melt adhesive film containing the anti-scratch coating comprises the following steps: coating the anti-scratch coating on the surface of the modified EVA adhesive film to obtain the hot melt adhesive film containing the anti-scratch coating; The hydroxyl value of the hydroxy acrylate is 110-135 mgKOH / g, and the solid content is 40-65%; The specific surface area of ​​the nano-silicon dioxide is 400-600m 2 / g, and the primary particle size is 12-18nm.

2. The hot melt adhesive film with anti-scratch coating according to claim 1, characterized in that: The EVA is one or more of EVA250, EVA550, and EVA650.

3. The hot melt adhesive film with anti-scratch coating according to claim 1, characterized in that: The coupling agent is one of a silane coupling agent and a titanate coupling agent.

4. The hot melt adhesive film with anti-scratch coating according to claim 1, characterized in that: The antioxidant is one of hindered phenol antioxidants, hindered amine antioxidants or phosphite antioxidants.

Citation Information

Patent Citations

  • Scratch resistant sub-gloss pre-coated film and preparation method thereof

    CN103965799A