Nickel alloy powder, conductive paste and multilayer ceramic capacitor

By forming an oxygen group compound film on the surface of the nickel powder and adding reinforced phase elements, the problem of sintering temperature drop caused by the reduction of nickel powder particle size is solved, the stability and cofiring of nickel powder are improved, and the multi-layer ceramic capacitors are satisfied. High performance requirements.

CN115240896BActive Publication Date: 2024-11-12NINGBO GUANGXIN NANOMATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210815730.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-11-12
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

In multi-layer ceramic capacitors, the reduction in the particle size of nickel powder leads to a decrease in the sintering temperature, resulting in poor expansion and contraction of the dielectric layer and the conductive layer at high temperatures, resulting in excessive sintering, aggregation, powder particle growth and conductor discontinuity, which in turn causes resistance Due to rising value and structural problems, existing improvement methods cannot meet high-performance requirements.

Method used

Using nickel alloy powder, the initial sintering temperature and stability of nickel powder are improved by forming an oxygen group compound film on the surface of nickel powder and adding elements that form a reinforced phase with nickel and the second main group element, and improving dielectric co-firedness and bonding of layers.

Benefits of technology

It effectively improves the initial sintering temperature and stability of nickel powder, extends service life, improves the cofiring and bonding of nickel powder with conductive paste and dielectric ceramic materials, and reduces the problems of rising resistance value and structural deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115240896B_ABST
    Figure CN115240896B_ABST
Patent Text Reader

Abstract

The invention discloses a nickel alloy powder, a conductive paste and a multilayer ceramic capacitor. The nickel alloy powder comprises, by mass percentage, 0.001-0.1% of an element forming a strengthening phase with nickel, 0.001-0.1% of a second main group element and 0.1-15% of an oxygen group element; the surface of the nickel alloy powder has an oxygen group element compound film, and the oxygen group element compound film comprises Ni a X b 、Ni c (XH) d 、Ni e C f X g The elements added to the nickel alloy powder of the present invention that form a strengthening phase with nickel effectively improve the initial sintering temperature of the nickel powder; the added second main group elements effectively improve the stability of the nickel powder, so that the use effect and service life of the nickel powder are improved; the added oxygen group elements form an oxygen group element compound film on the surface of the nickel powder, which has a good protective effect on the added elements inside the nickel powder, and improves the co-firing and mutual bonding of the nickel powder with the glass powder in the conductive paste and the dielectric ceramic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal powders, and more specifically, to nickel alloy powder, conductive paste and multilayer ceramic capacitors. Background Art

[0002] The metal conductive powder is evenly mixed with glass dielectric adhesive or other additives and dispersed in an organic carrier to make a conductive paste. The conductive paste and the dielectric layer are then alternately stacked repeatedly through a printing process and fired at a high temperature to form a multi-layer ceramic capacitor.

[0003] In the past, precious metals such as palladium, silver, and platinum were mostly used as internal electrode materials for multilayer ceramic capacitors. However, oxidation expansion during sintering of palladium or silver-palladium will cause delamination, cracking, and other problems. In order to save resources, base metals such as nickel have gradually become the main conductive powder in conductive pastes.

[0004] As the number of layers of multilayer ceramic capacitors increases (more than 100 layers), the thickness of each layer is also getting thinner (less than 3 microns), and the particle size of the nickel powder used is also getting smaller (10 to 1000nm). As the particle size of nickel powder continues to decrease, the sintering temperature of nickel powder is also showing a downward trend. However, the sintering temperature of the dielectric layer is much higher than the sintering temperature of nickel powder. At high temperatures, the dielectric layer and the conductive layer cannot expand and contract well together, which will lead to excessive sintering of nickel powder, and then produce nickel aggregation, powder growth, and conductor discontinuity. This will not only lead to the problem of increased resistance value, but also cause problems such as breakage and deformation.

[0005] Changing the surface morphology of nickel powder by conventional physical methods and improving the dispersibility of nickel powder by fluid dispersion can no longer meet the needs of high-performance multilayer ceramic capacitors. Nickel alloy powder obtained by adding any one or more elements of vanadium, chromium, zirconium, niobium, molybdenum, tantalum and tungsten to nickel powder can increase the initial sintering temperature of conductive paste. However, the above elements are easy to react with the ceramic material of the dielectric layer and have an adverse effect on the conductivity of the multilayer ceramic capacitor electrode.

[0006] Therefore, how to effectively improve the performance of nickel powder used in multilayer ceramic capacitors has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0007] An object of the present invention is to provide a new technical solution for nickel alloy powder which effectively improves the performance of nickel powder for multilayer ceramic capacitors.

[0008] According to a first aspect of the present invention, a nickel alloy powder is provided.

[0009] The nickel alloy powder comprises, by mass percentage, 0.001-0.1% of an element forming a strengthening phase with nickel, 0.001-0.1% of a second main group element and 0.1-15% of an oxygen group element;

[0010] The surface of the nickel alloy powder has a chalcogen compound film, and the chalcogen compound film includes Ni a X b 、Ni c (XH) d 、Ni e C f X g and H2X, and Ni a X b 、Ni c (XH) d 、Ni e C f X g The ratio of the sum of the oxygen group element atomic concentrations in H2X to the total oxygen group element atomic concentration in the nickel alloy powder is greater than 70%, and the ratio of the oxygen group element atomic concentration in H2X to the total oxygen group element atomic concentration in the nickel alloy powder is greater than 0 and less than or equal to 30%, wherein X is an oxygen group element, and the value ranges of a, b, c, d, e, f, and g are all 1-3.

[0011] Optionally, the element that forms a strengthening phase with nickel includes at least one of aluminum, silicon, titanium, zirconium, hafnium, vanadium, niobium and tantalum.

[0012] Optionally, the ratio of the sum of the concentrations of oxygen group atoms within a thickness of 5 nm from the outside to the inside of the nickel alloy powder to the total concentration of oxygen group atoms in the nickel alloy powder is greater than 50%.

[0013] Optional, Ni a X b 、Ni c (XH) d The ratio of the sum of the atomic concentrations of the oxygen group elements in the nickel alloy powder to the total atomic concentration of the oxygen group elements in the nickel alloy powder is greater than 40%.

[0014] Optionally, the nickel alloy powder has a flaky, spherical or quasi-spherical morphology.

[0015] According to a second aspect of the present invention, a conductive paste is provided.

[0016] The conductive paste includes the nickel alloy powder of the present invention.

[0017] Optionally, when the average particle size d of the nickel alloy powder is 10-100 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 100;

[0018] When the average particle size d of the nickel alloy powder is 101-200 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 50;

[0019] When the average particle size d of the nickel alloy powder is 201-1000 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 25.

[0020] Optionally, the degree of discreteness of the observed particle size d1 of the nickel alloy powder within the field of view of a preset scanning electron microscope imaging range is expressed by a range R, and R=Max(d1)-Min(d1), wherein R:d>2, and d is the average particle size of the nickel alloy powder.

[0021] According to a third aspect of the present invention, a multilayer ceramic capacitor is provided.

[0022] The multilayer ceramic capacitor comprises electrodes formed by the conductive paste of the present invention.

[0023] The elements added to the nickel alloy powder of the present invention that form a strengthening phase with nickel effectively improve the initial sintering temperature of the nickel powder; the added second main group elements effectively improve the stability of the nickel powder, thereby improving the use effect and service life of the nickel powder; the added oxygen group elements form an oxygen group element compound film on the surface of the nickel powder, which has a good protective effect on the added elements inside the nickel powder, and improves the co-firing and mutual bonding degree of the nickel powder with the glass powder in the conductive paste and the dielectric ceramic material.

[0024] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.

[0026] Figure 1 It is a comparison chart of the dispersibility test of Example 1 and Comparative Example 1.

[0027] Figure 2 This is the TGA chart of Example 3.

[0028] Figure 3 This is the TGA diagram of Comparative Example 3. DETAILED DESCRIPTION

[0029] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values ​​set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.

[0030] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.

[0031] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.

[0032] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0033] The nickel alloy powder provided by the present invention includes, by mass percentage, 0.001-0.1% of an element that forms a strengthening phase with nickel, 0.001-0.1% of a second main group element, and 0.1-15% of an oxygen group element. The average particle size d of the nickel alloy powder converted according to the BET specific surface area can be 10-1000nm. The second main group element can be at least one of beryllium, magnesium, calcium, strontium and barium. The oxygen group element can be at least one of oxygen, sulfur, selenium and tellurium.

[0034] The surface of the nickel alloy powder has a chalcogen compound film, which includes Ni a X b 、Ni c (XH) d 、Ni e C f X g and H2X, and Ni a X b 、Ni c (XH) d 、Ni e C f X g The ratio of the sum of the concentration of oxygen group atoms in the H2X to the total concentration of oxygen group atoms in the nickel alloy powder is greater than 70%, and the ratio of the concentration of oxygen group atoms in H2X to the total concentration of oxygen group atoms in the nickel alloy powder is greater than 0 and less than or equal to 30%. X is an oxygen group element, and the value range of a, b, c, d, e, f, and g is 1-3. The specific values ​​of a, b, c, d, e, f, and g are determined by the valence of each component element of the compound.

[0035] The nickel alloy powder of the invention has the characteristics of high initial oxidation temperature, good corrosion resistance, excellent co-firing property with a ceramic dielectric layer, better use effect and longer service life.

[0036] The elements added to the nickel alloy powder of the present invention that form a strengthening phase with nickel effectively improve the initial sintering temperature of the nickel powder; the added second main group elements effectively improve the stability of the nickel powder, thereby improving the use effect and service life of the nickel powder; the added oxygen group elements form an oxygen group element compound film on the surface of the nickel powder, which has a good protective effect on the added elements inside the nickel powder, and improves the co-firing and mutual bonding degree of the nickel powder with the glass powder in the conductive paste and the dielectric ceramic material.

[0037] In one embodiment of the nickel alloy powder of the present invention, the element forming a reinforcement phase with nickel includes at least one of aluminum, silicon, titanium, zirconium, hafnium, vanadium, niobium and tantalum.

[0038] In one embodiment of the nickel alloy powder of the present invention, the ratio of the sum of the concentration of chalcogen atoms within a thickness of 5 nm from the outside to the inside of the nickel alloy powder to the total concentration of chalcogen atoms in the nickel alloy powder is greater than 50%. The limitation in this embodiment is conducive to avoiding the problem of instability of nickel alloy crystals caused by excessive concentration of chalcogens in the 5 nm surface layer of non-nickel alloy powder.

[0039] In one embodiment of the nickel alloy powder of the present invention, Ni a X b 、Ni c (XH) d The ratio of the sum of the atomic concentrations of the oxygen group elements in the nickel alloy powder to the total atomic concentration of the oxygen group elements in the nickel alloy powder is greater than 40%. a X b 、Ni c (XH) d (Especially Ni a X b ) is conducive to better combination of nickel alloy powder and slurry system.

[0040] In one embodiment of the nickel alloy powder of the present invention, the nickel alloy powder has a flaky, spherical or quasi-spherical morphology.

[0041] The invention also provides a conductive paste comprising the nickel alloy powder of the invention.

[0042] In one embodiment of the conductive paste of the present invention, when the average particle size d of the nickel alloy powder is 10-100nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of the preset scanning electron microscope imaging range is less than or equal to 100; when the average particle size d of the nickel alloy powder is 101-200nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of the preset scanning electron microscope imaging range is less than or equal to 50; when the average particle size d of the nickel alloy powder is 201-1000nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of the preset scanning electron microscope imaging range is less than or equal to 25. The field of view in this embodiment can be, for example, 10 100d×75d fields of view randomly selected within the scanning electron microscope imaging range. The particle size distribution of the nickel alloy powder in this embodiment can effectively improve the uniformity and stability of the slurry.

[0043] Taking 300nm nickel alloy powder as an example, in 10 random SEM photos with a 4:3 ratio and a long side of the field of view of 30μm, the total number of nickel alloy powder particles that meet the condition of d1>1.2μm is no more than 25 through software analysis counting or manual statistics, which can be considered to meet the requirements of the present invention.

[0044] In one embodiment of the conductive paste of the present invention, the degree of dispersion of the observed particle size d1 of the nickel alloy powder within the field of view of the preset scanning electron microscope imaging range is represented by the range R, and R = Max (d1) - Min (d1), wherein R: d> 2, d is the average particle size of the nickel alloy powder. The field of view in this embodiment can be, for example, 10 60d × 45d fields of view randomly selected within the scanning electron microscope imaging range. The particle size distribution of the nickel alloy powder in this embodiment can effectively improve the uniformity and stability of the slurry.

[0045] The present invention also provides a multilayer ceramic capacitor comprising electrodes formed by the conductive paste of the present invention.

[0046] The experimental methods used in the following examples are all conventional methods unless otherwise specified. The materials and reagents used are all commercially available unless otherwise specified. The equipment used in the experiments are all well known to those skilled in the art unless otherwise specified.

[0047] The nickel alloy powders in the embodiments of the present invention are all prepared by a physical vapor evaporation condensation method, and the added elements that form a strengthening phase with nickel and the second main group elements evaporate simultaneously with the nickel in the same high-temperature evaporator, and are accompanied by nickel vapor nucleation, growth, crystallization and solidification to form nickel alloy powder, and a chalcogen compound film is formed on the surface of the nickel alloy powder by a chemical method (for example, by mixing chalcogens and nickel alloy powder under high temperature conditions, a chalcogen compound film can be formed on the surface of the nickel alloy powder).

[0048] Example 1

[0049] The nickel alloy powder of this embodiment has an average particle size of 385nm converted from the specific surface area measured by the BET method; the elements added to form a strengthening phase with nickel are zirconium and silicon, and the weight content of zirconium added is controlled to be 0.025%, and the weight content of silicon is controlled to be 0.003%; the second main group element added is calcium, which is used to strengthen the alloy grain boundary and improve the use effect of the alloy powder, and the weight content of calcium added is controlled to be 0.015%; the oxygen group elements added are oxygen and sulfur, and the weight content of oxygen is controlled to be 1.05%, and the weight content of sulfur is controlled to be 0.075%. Through XPS surface element analysis, the oxygen group elements in the nickel alloy powder are mainly NiO, Ni(OH)2, CO (forming the compound Ni e C f X g ), NiS, H2O and H2S, among which the sum of the atomic concentrations of the oxygen group elements of NiO, Ni(OH)2, CO and NiS accounts for 93% of the total atomic concentration of the oxygen group elements, and the sum of the atomic concentrations of the oxygen group elements of H2O and H2S accounts for 7% of the total atomic concentration of the oxygen group elements.

[0050] Comparative Example 1

[0051] The preparation process of the nickel powder of Comparative Example 1 is the same as that of Example 1, but no element forming a strengthening phase with nickel and the second main group element are added, and no oxygen group element compound film is formed on the surface. The average particle size of the obtained nickel powder converted by the specific surface area measured by the BET method is 365nm.

[0052] The nickel alloy powder prepared in Example 1 and the nickel powder prepared in Comparative Example 1 were exposed to air with a humidity of 60% at room temperature. Samples were taken after 24 hours, 15 days and 30 days respectively. The powders were placed in alcohol and stirred under the same conditions and then scraped to test the soft agglomeration of the powders. Figure 1 As shown, after 24 hours, the dispersion of the powders of Example 1 and Comparative Example 1 in the scraping test was similar, and no obvious agglomeration occurred; after 15 days, the dispersion of the powders of Example 1 and Comparative Example 1 in the scraping test was quite different, the nickel alloy powder of Example 1 still maintained good dispersion, and the nickel powder of Comparative Example 1 had obvious agglomeration; after 30 days, the nickel alloy powder of Example 1 had slight agglomeration, and the agglomeration of the powder of Comparative Example 1 was more serious than the test result on the 15th day, and larger agglomerates began to appear. It can be seen from the test that the nickel alloy powder of Example 1 has improved stability and service life compared with Comparative Example 1.

[0053] Example 2

[0054] The nickel alloy powder of this embodiment has an average particle size of 977nm converted by specific surface area measured by BET method; wherein the element added to form a strengthening phase with nickel is aluminum, and the weight content of the added aluminum is controlled to be 0.012%; the second main group element added is magnesium, which is used to strengthen the alloy grain boundary and improve the use effect of the alloy powder, and the weight content of the added magnesium is controlled to be 0.009%; the oxygen group elements added are oxygen and selenium, and the weight content of oxygen is controlled to be 0.15%, and the weight content of selenium is controlled to be 0.005%. Through XPS surface element analysis, the oxygen group elements in the nickel alloy powder mainly exist in the form of NiO, Ni(OH)2, CO, NiSe2 and H2O, wherein the sum of the atomic concentrations of oxygen group elements of NiO, Ni(OH)2, CO and NiSe2 accounts for 96% of the total atomic concentrations of oxygen group elements, and the sum of the atomic concentrations of oxygen group elements of H2O accounts for 3% of the total atomic concentrations of oxygen group elements.

[0055] Comparative Example 2

[0056] The preparation process of the nickel powder in this comparative example 2 is the same as that in Example 2, but no element forming a strengthening phase with nickel and the second main group element are added, and no oxygen group element compound film is formed on the surface. The average particle size of the obtained nickel powder converted by the specific surface area measured by the BET method is 946nm.

[0057] The nickel alloy powder prepared in Example 2 and the nickel powder in Comparative Example 2 were made into a conductive paste, and the conductive paste was used to make a multilayer ceramic capacitor. By counting the yield rate of the multilayer ceramic capacitors prepared by the samples (defective products that have warped and deformed to cause short circuits), each thousand ceramic capacitors were a group, and the number of defective products in three groups was counted, as shown in Table 1, it was found that the addition of the nickel alloy powder in Example 2 improved the co-firing and bonding with the dielectric ceramic, and reduced the defective rate of the warped capacitors.

[0058] Table 1

[0059]

[0060] Example 3

[0061] The nickel alloy powder of this embodiment has an average particle size of 95nm converted by specific surface area measured by BET method; wherein the elements added to form strengthening phase with nickel are hafnium and titanium, and the weight content of hafnium added is controlled to be 0.015%, and the weight content of titanium added is controlled to be 0.001%; ​​the second main group element added is barium element, which is used to strengthen the alloy grain boundary and improve the use effect of the alloy powder, and the weight content of barium added is controlled to be 0.033%; the oxygen group element added is oxygen, and the weight content of oxygen element is controlled to be 7.45%. Through XPS surface element analysis, the oxygen group elements in the nickel alloy powder mainly exist in the form of NiO, Ni(OH)2, CO and H2O, wherein the sum of the atomic concentrations of oxygen group elements of NiO and Ni(OH)2 accounts for 41% of the total atomic concentrations of oxygen group elements, the atomic concentrations of oxygen group elements of CO accounts for 31% of the total atomic concentrations of oxygen group elements, and the sum of the atomic concentrations of oxygen group elements of H2O accounts for 27% of the total atomic concentrations of oxygen group elements.

[0062] Comparative Example 3

[0063] The preparation process of the nickel powder of this comparative example 3 is the same as that of Example 3, but no element forming a strengthening phase with nickel and the second main group element are added, and no oxygen group element compound film is formed on the surface. The average particle size of the obtained nickel powder converted by the specific surface area measured by the BET method is 89nm.

[0064] The sintering conditions of the nickel alloy powder of Example 3 and the nickel powder of Comparative Example 3 were tested by TMA (thermomechanical analysis). The powder was made into a block sample with a length, width and height of 4*4*2, and heated at a heating rate of 10°C / min in nitrogen protection, while the shrinkage of the sample block height was tested. From the starting deformation temperature obtained from the obtained TMA graph, it was found that the starting sintering temperature of the nickel alloy powder of Example 3 was increased by 18.5°C compared with the nickel powder of Comparative Example 3.

[0065] The weight change of the powder in an oxygen atmosphere during the heating process is detected by TGA (thermal gravimetric analysis) to confirm the starting oxidation temperature. Figure 2 It can be seen that the initial oxidation temperature of the nickel alloy powder prepared in Example 3 is 411°C. Figure 3 It can be seen that the initial oxidation temperature of the nickel powder prepared in Comparative Example 3 is 389°C, that is, the initial oxidation temperature of the nickel alloy powder of Example 3 is increased by 22°C compared with the nickel powder of Comparative Example 3.

[0066] Example 4

[0067] The nickel alloy powder of this embodiment has an average particle size of 16nm converted from the specific surface area measured by the BET method; wherein the elements added to form a strengthening phase with nickel are vanadium and tantalum, and the weight content of the added vanadium is controlled to be 0.015%, and the weight content of the added tantalum is controlled to be 0.001%; ​​the second main group element added is beryllium, which is used to strengthen the alloy grain boundary and improve the use effect of the alloy powder, and the weight content of the added beryllium is controlled to be 0.097%; the added oxygen group element is oxygen, and the weight content of the oxygen element is controlled to be 2.76%. Through XPS surface element analysis, the oxygen group elements in the nickel alloy powder mainly exist in the form of NiO, Ni(OH)2, CO, etc., wherein the sum of the atomic concentrations of the oxygen group elements of NiO and Ni(OH)2 accounts for 67% of the total atomic concentrations of the oxygen group elements.

[0068] Example 5

[0069] The nickel alloy powder of this embodiment has an average particle size of 694nm converted from the specific surface area measured by the BET method; wherein the element added to form a strengthening phase with nickel is niobium, and the weight content of the added niobium is controlled to be 0.004%; the second main group element added is strontium, which is used to strengthen the alloy grain boundary and improve the use effect of the alloy powder, and the weight content of the added strontium is controlled to be 0.017%; the oxygen group element added is oxygen, and the weight content of the oxygen element is controlled to be 0.109%. Through XPS surface element analysis, the oxygen group elements in the nickel alloy powder mainly exist in the form of NiO, Ni(OH)2, CO and H2O, wherein the sum of the oxygen group element atomic concentrations of NiO and Ni(OH)2 accounts for 77.1% of the total oxygen group element atomic concentration, the oxygen group element atomic concentration of CO accounts for 21.3% of the total oxygen group element atomic concentration, and the sum of the oxygen group element atomic concentration of H2O accounts for 0.6% of the total oxygen group element atomic concentration.

[0070] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.

Claims

1. A nickel alloy powder, characterized in that: The composition comprises, by mass percentage, 0.001-0.1% of an element that forms a strengthening phase with nickel, 0.001-0.1% of a second main group element, and 0.1-15% of an oxygen group element; The surface of the nickel alloy powder has a chalcogen compound film, and the chalcogen compound film includes Ni a X b 、Ni c (XH) d 、Ni e C f X g and H2X, and Ni a X b 、Ni c (XH) d 、Ni e C f X g The ratio of the sum of the oxygen group element atomic concentrations in H2X to the total oxygen group element atomic concentration in the nickel alloy powder is greater than 70%, and the ratio of the oxygen group element atomic concentration in H2X to the total oxygen group element atomic concentration in the nickel alloy powder is greater than 0 and less than or equal to 30%, wherein X is an oxygen group element, and the value ranges of a, b, c, d, e, f, and g are all 1-3.

2. The nickel alloy powder according to claim 1, characterized in that The element that forms a strengthening phase with nickel includes at least one of aluminum, silicon, titanium, zirconium, hafnium, vanadium, niobium and tantalum.

3. The nickel alloy powder according to claim 1, characterized in that The ratio of the sum of the concentration of oxygen group elements atoms within a thickness of 5 nm from the outside to the inside of the nickel alloy powder to the total concentration of oxygen group elements atoms in the nickel alloy powder is greater than 50%.

4. The nickel alloy powder according to claim 1, characterized in that Ni a X b 、Ni c (XH) d The ratio of the sum of the atomic concentrations of the oxygen group elements in the nickel alloy powder to the total atomic concentration of the oxygen group elements in the nickel alloy powder is greater than 40%.

5. The nickel alloy powder according to claim 1, characterized in that The nickel alloy powder has a flaky, spherical or quasi-spherical shape.

6. A conductive paste, characterized in that: The nickel alloy powder comprises the nickel alloy powder as claimed in any one of claims 1 to 5.

7. The conductive paste according to claim 6, characterized in that: When the average particle size d of the nickel alloy powder is 10-100 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 100; When the average particle size d of the nickel alloy powder is 101-200 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 50; When the average particle size d of the nickel alloy powder is 201-1000 nm, the number of particles of the nickel alloy powder with an observed particle size d1 greater than 4d within the field of view of a preset scanning electron microscope imaging range is less than or equal to 25.

8. The conductive paste according to claim 6, characterized in that: The degree of dispersion of the observed particle size d1 of the nickel alloy powder within the field of view of the preset scanning electron microscope imaging range is represented by the range R, and R=Max(d1)-Min(d1), wherein R:d>2, d is the average particle size of the nickel alloy powder.

9. A multilayer ceramic capacitor, characterized in that: An electrode formed from the conductive paste according to any one of claims 6 to 8.

Citation Information

Patent Citations

  • Nickel powder, conductive paste, and multilayer electronic component using same

    CN100565713C

  • Nickel powder, method for manufacturing same, conductor paste, and multilayer ceramic electronic component using same

    CN101264523A

  • Nickel powder or alloy powder having nickel as main component, method for manufacturing the powder, conductive paste and laminated ceramic capacitor

    CN101808767A

  • Device for achieving continuous mass production of high-purity nanoscale metal particles through circulation cooling

    CN106735279A

  • Surface treatment method for superfine metal nickel powder

    CN109648093A