Method for coating battery negative electrode sheet safety layer slurry and battery negative electrode sheet

By controlling the solid content and viscosity of the safety layer slurry, combined with twin-screw stirring and extrusion coating technology, the existing technology solves the problems of cumbersome safety coating procedures on the surface of the pole pieces and affecting the energy density, and realizes lithium-ion batteries. Thin security layer and good security.

CN115275114BActive Publication Date: 2024-10-29SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211007709.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-22
Publication Date
2024-10-29
Estimated Expiration
2042-08-22

AI Technical Summary

Technical Problem

Among the existing safety improvement measures for lithium-ion batteries, flame-retardant electrolyte technology has made slow progress, and the technical process of safety coating on the surface of pole pieces is cumbersome and difficult to achieve a thin safety coating, which affects the energy density and safety of the battery.

Method used

Use a safety layer slurry with a solid content of 3-10% and a viscosity of 50-200CP, prepare it through twin-screw stirring, and perform extrusion coating on the basis of active material layer coating. Adjust the die gap and gasket thickness to achieve Thin and even application of safety layer.

Benefits of technology

Without affecting the energy density of the battery, a thin safety layer thickness and good safety are achieved, improving the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115275114B_ABST
    Figure CN115275114B_ABST
Patent Text Reader

Abstract

The invention provides a method for coating a safety layer slurry of a battery negative electrode sheet, including safety layer slurry preparation, extrusion coating and drying, wherein the safety layer slurry preparation is to mix and stir a carboxymethyl cellulose binder with pure water to form a CMC glue solution, and the CMC glue solution is mixed and stirred evenly with a safety solute and a polyacrylonitrile binder in a twin-screw mixer to obtain a safety layer slurry having a solution solid content of 3-10% and a viscosity of 50-200CP; extrusion coating is to coat the safety layer slurry on the basis of coating an active material layer slurry, wherein the active material layer slurry is coated between a coated foil and the safety layer slurry, and during coating, the distance between the coating die head of the safety layer slurry and the active material layer is 100-300μm, and the thickness of the gasket at the outlet of the safety layer slurry is 0.1-0.3mm. The invention limits the solid content and viscosity of the safety layer slurry, the gap between the coating die head and the thickness of the gasket, so that the safety layer coated by the method can have a thin thickness and good safety without affecting the energy density of the electrode sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemistry, and in particular to a method for coating a safety layer slurry on a battery negative electrode sheet. The present invention also relates to a battery negative electrode sheet prepared by the method. Background Art

[0002] The number of lithium-ion power batteries installed in vehicles is increasing year by year, and the market share of power battery vehicles is also increasing; more and more companies are entering the power battery manufacturing industry, resulting in increasing competition pressure and higher market barriers. At present, in order to increase the energy density of power batteries, most companies have begun to use high nickel + silicon carbon system to prepare lithium-ion power batteries. However, high energy density also comes with high risk; the current measures to improve battery safety mainly include the use of flame-retardant electrolytes, diaphragm safety coating technology, pole piece surface safety coating and other technologies.

[0003] Flame-retardant electrolyte technology has made slow progress in the industry. The main reason is that the amount of flame retardant is not easy to control. If too little flame retardant is added, it cannot play a role in improving safety. If too much flame retardant is added, it will affect the battery's electrical properties such as cycle, internal resistance, and rate, especially the electrolyte design battery chemical reaction and kinetics. There has been no major technological breakthrough in the industry, causing this technology to remain in the laboratory stage. Compared with the diaphragm safety coating technology, the pole surface safety coating technology is safer because there is a gap between the diaphragm and the pole when the battery fails (lithium-ion battery failure refers to abnormal battery operation due to certain specific material reasons, such as a short circuit in the battery). The diaphragm cannot form a stable protection for the pole, and the safety pole coating and the pole's conductive material layer fit tightly. The pole surface safety coating technology is currently the simplest, lowest manufacturing cost, and best technology for improving battery safety.

[0004] The micro-concave coating technology in the surface safety coating technology is to carry out multi-layer coating in multiple times. After each layer of coating is completed, it needs to be baked, dried and rolled up, and then re-rolled for the next coating and baking. The process is cumbersome, the coating efficiency is low, the equipment purchase cost is increased, and the foil is baked multiple times to reduce its strength. Roller breaking problems are prone to occur. The process of using multiple layers of coating at the same time is more advantageous, but the thickness of the safety coating when the existing technology is applied simultaneously is thicker, and the thicker safety coating is likely to affect the energy density of the electrode. Due to the influence of various factors, it is difficult to achieve a thinner safety coating in the industry, especially the multi-layer coating technology that is extruded once with more than two systems of negative electrode materials is a process solution that is more difficult to achieve in the industry. Summary of the invention

[0005] In view of this, the present invention proposes a method for coating a safety layer slurry of a battery negative electrode sheet. The negative electrode sheet safety layer coated by the method of the present invention can make the electrode sheet have a thinner thickness and good safety without affecting the energy density.

[0006] A method for coating a safety layer slurry on a negative electrode sheet of a battery comprises safety layer slurry preparation, extrusion coating and drying, wherein the safety layer slurry preparation comprises mixing a carboxymethyl cellulose binder with pure water to form a CMC glue solution, and the CMC glue solution is mixed and stirred evenly with a safety solute and a polyacrylonitrile binder in a twin-screw mixer, wherein the safety layer slurry has a solution solid content of 3-10% and a viscosity of 50-200 CP; wherein the extrusion coating comprises coating the safety layer slurry on the basis of coating the active material layer slurry, wherein the active material layer slurry is coated between a foil material 3 to be coated and the safety layer slurry, wherein during coating, the distance between the coating die head of the safety layer slurry and the active material layer is 100-300 μm, and the thickness of the safety layer slurry outlet gasket is 0.1-0.3 mm.

[0007] Furthermore, the safety layer slurry preparation includes the following steps: preparing CMC glue: adding carboxymethyl cellulose binder and pure water into a glue tank, using a PD mixer to stir for multiple times, setting the twist paddle to stir at a low speed of 15-30rpm for 10-45min for the first time; setting the twist paddle at a speed of 20-35rpm and the biaxial dispersion disk at a speed of 1000-3000rpm for the second time, and stirring for 30-60min at the same time; setting the twist paddle at a speed of 25-35rpm and the biaxial dispersion disk at a speed of 2000-3000rpm for the third time, ... 00rpm, stirring for 150-240min, and controlling the vacuum in the range of -90-99kPa to obtain the CMC glue solution; twin-screw stirring: adding the CMC glue solution to the first feeding port of the twin-screw mixer, rotating at a speed of 10-100rpm, adding the safety solute and polyacrylonitrile adhesive to the second and third feeding ports respectively, rotating at a speed of 10-100rpm, and high-speed sand grinding and stirring at a speed of 1000-3000rpm; after vacuum defoaming, the safety layer slurry is obtained.

[0008] Furthermore, in the raw materials for preparing the safety layer slurry, the weight ratio of carboxymethyl cellulose binder, polyacrylonitrile binder and safety solute is (0.5-2):(1-5):(87-97), and the safety solute includes at least one of boehmite and silica.

[0009] Furthermore, the weight ratio of silicon-carbon material, conductive carbon black, polyacrylonitrile binder, carboxymethyl cellulose binder and styrene-butadiene rubber binder in the raw materials for preparing the active material layer slurry is (90-98): (0.5-5): (0.5-3): (0.5-2): (0.5-2.5).

[0010] Furthermore, the silicon-carbon material includes graphite and silicon-oxygen material, wherein the silicon-oxygen material accounts for 3-30% of the silicon-carbon material.

[0011] Furthermore, the opening width of the safety layer slurry outlet gasket is 2-4 mm smaller than the opening width of the active material layer slurry outlet gasket.

[0012] Furthermore, the chamfer of the safety layer slurry outlet gasket in the opening direction is smaller than that in the depth direction.

[0013] Furthermore, the chamfer of the safety layer slurry outlet gasket in the opening direction is 3*5mm, 3*4mm, 2*4mm or 2*5mm.

[0014] Furthermore, the drying includes the following steps: in the first stage, the temperature is set at 70-85°C and the wind frequency is 10-20Hz for baking; in the second stage, the temperature is set at 70-85°C and the wind frequency is 20-40Hz for baking; in the third stage, the temperature is set at 55-70°C and the wind frequency is 10-20Hz for baking.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] The coating method of the present invention can make the safety layer thinner after drying, and the coating uniformity and consistency are better by using a safety layer slurry with a solid content of 3-10% and a viscosity of 50-200CP. During coating, the die gap is adjusted to 100-300μm, and the thickness of the safety layer slurry outlet gasket is 0.1-0.3mm. When the safety layer is thinner, the diffusion of the safety layer slurry is more spread out and it is easier to cover the active material layer. The present invention further preferably adopts a twin-screw stirring preparation process, which can make the prepared safety layer slurry more dispersible, uniform and consistent. The safety layer coated by this method can make the pole piece have a thinner thickness and good safety without affecting the energy density.

[0017] The present invention also provides a battery negative electrode sheet prepared by adopting the above-mentioned method for coating the battery negative electrode sheet safety layer slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0019] Figure 1 is a flow chart of the coating method of the present invention;

[0020] Figure 2 This is a cross-sectional SEM image of the safety layer of Example 1 of the present invention;

[0021] Figure 3 This is a cross-sectional SEM image of the safety layer of Example 2 of the present invention;

[0022] Figure 4 This is a cross-sectional SEM image of the safety layer of Example 3 of the present invention;

[0023] Figure 5 This is a cross-sectional SEM image of the safety layer of Example 4 of the present invention;

[0024] Figure 6 This is a cross-sectional SEM image of the safety layer of Comparative Example 1 of the present invention;

[0025] Figure 7 This is a cross-sectional SEM image of the safety layer of Comparative Example 2 of the present invention;

[0026] Figure 8 This is a cross-sectional SEM image of the safety layer of Comparative Example 3 of the present invention;

[0027] Fig. 9 This is a cross-sectional SEM image of the safety layer of Comparative Example 4 of the present invention;

[0028] Fig.10 This is a SEM image of the surface of the safety layer of Example 1 of the present invention;

[0029] Fig.11 This is a SEM image of the safety layer surface of Comparative Example 4 of the present invention;

[0030] Fig.12 It is a schematic diagram of the coating stage in the coating method of the present invention;

[0031] Fig.13 It is a schematic diagram of the coating stage in the coating method of the present invention from another perspective.

[0032] Description of reference numerals:

[0033] 1. Single-layer extrusion die; 2. Multi-layer extrusion die; 3. Foil; 4. Coating roller. DETAILED DESCRIPTION

[0034] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0035] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from conventional biochemical reagent stores unless otherwise specified. In addition, except for special instructions in this example, the terms and processes involved in this example are understood according to the general knowledge and conventional methods in the prior art.

[0036] A method for coating a safety layer slurry on a negative electrode sheet of a battery comprises the following steps: preparing the safety layer slurry, extrusion coating and drying, wherein the safety layer slurry is prepared by mixing a carboxymethyl cellulose binder with pure water to form a CMC glue solution, and the CMC glue solution is uniformly mixed and stirred with a safety solute and a polyacrylonitrile binder in a twin-screw mixer, wherein the safety layer slurry has a solution solid content of 3-10% and a viscosity of 50-200 CP; and extrusion coating is performed on the basis of coating an active material layer slurry, wherein the active material layer slurry is coated between a foil material 3 to be coated and the safety layer slurry, and during coating, the gap between the coating die head of the safety layer slurry and the coating die head of the active material layer slurry is 100-300 μm, and the thickness of the safety layer slurry outlet gasket is 0.1-0.3 mm.

[0037] The coating method of the present invention adopts a safety layer slurry with a solid content of 3-10% and a viscosity of 50-200CP, which can make the safety layer after drying thinner, and the coating uniformity and consistency are better. During coating, the die gap is adjusted to 50-130μm, and the thickness of the safety layer slurry outlet gasket is 0.1-0.3mm. When the safety layer is thinner, the diffusion of the safety layer slurry is more spread out and it is easier to cover the active material layer. The present invention further adopts twin-screw stirring, which can make the prepared safety layer slurry more dispersible, uniform and consistent. The safety layer coated by the present invention can make the pole piece have a thinner thickness and good safety without affecting the energy density.

[0038] Based on the above design concept, in order to improve the coating efficiency, the present invention adopts a multi-layer extrusion coating die to coat the active material layer slurry, such as Figure 1 As shown, the active material layer slurries of different systems are prepared in separate tanks in the slurry mixing tank, and are placed in storage tanks for buffer storage and are reserved for coating. Fig.12 and Fig.13As shown, after the foil 3 is unwound on the coating roller 4, the cached active material layer slurry is pumped to the multilayer extrusion die 2 and coated at the same time. Then, the safety layer slurry is coated on the basis of the coating of the active material layer slurry, and the coating of the safety layer slurry is carried out by a single-layer extrusion die 1. A gasket is installed in the nozzle of each layer of the extrusion coating die, and the slurry is sprayed out from the die through the blank gap of the gasket and coated on the surface of the foil. The foil forms a wrapped arc on the coating roller, and moves unidirectionally as the coating roller rotates in situ. When passing through the adjustable coating die set at a fixed position, the slurry is sprayed onto the surface of the foil to complete the coating. The multilayer extrusion die 2 usually uses an extruder for extrusion, so that the slurry passes through the extrusion die and is evenly coated on the foil 3 at a designed speed and thickness. After the coating is completed, it is baked in an oven, and the electrode is obtained after the slurry is dried, and then rolled up.

[0039] In detail, in the safety layer slurry preparation stage, the preferred safety layer slurry preparation raw materials of the present invention have a weight ratio of (0.5-2): (1-5): (87-97). CMC and polyacrylonitrile binder are used as binders to play a role of fixed bonding. CMC can specifically use carboxymethyl cellulose sodium binder, and polyacrylonitrile binder can use commercially available polyacrylonitrile multi-polymer water-based binder; the safety solute has a certain electronic insulation effect and can increase the safety performance of the battery. The safety solute preferably includes at least one of boehmite and silica. In addition to the above raw materials, the safety layer slurry usually also has pure water, which is used as a solvent to play a role of dilution and dissolution. In order to make the safety layer slurry more uniform, it is well known that additives containing alcohol groups can be added to reduce the specific surface area of ​​the particles, improve the degree of dispersion, and reduce slurry agglomeration.

[0040] The raw materials for preparing the active material layer slurry include silicon-carbon material, conductive carbon black, polyacrylonitrile binder, carboxymethyl cellulose binder and styrene-butadiene rubber binder in a weight ratio of (90-98): (0.5-5): (0.5-3): (0.5-2): (0.5-2.5). Silicon-carbon material is the main component of the active material layer slurry, which is used to improve the energy density of the battery. The silicon-carbon material is composed of high-gram capacity graphite mixed with silicon oxygen or silicon, wherein the preferred silicon oxygen material accounts for 3-30% of the silicon-carbon material, and the graphite can be at least one of artificial graphite and natural graphite. The viscosity of the active material layer slurry usually needs to be controlled within the range of 3000-10000CP, and the solid content usually needs to be controlled within the range of 45%-60%.

[0041] The preparation of the active material layer slurry can be carried out by conventional means in the art, which will not be described in detail here. In order to make the safety layer slurry more uniform, the present invention further recommends the following method for preparing the safety layer slurry.

[0042] In the preparation process of the safety layer slurry, in order to make CMC fully dissolved, a wet mixing process is used, and the material dosage is calculated so that the volume of CMC glue is 50%-80% of the volume of the slurry tank. Specifically, the following steps can be preferably included: first, pure water is added to the glue tank, and then an appropriate amount of CMC powder is added. After the CMC powder is added, it is slowly stirred to sink the powder into the pure water; wherein CMC accounts for 0.5-3%. The glue is stirred in three steps using a PD mixer: the first time, the twist paddle is set to stir at a low speed of 15-30rpm for 10-45min; the second time, the twist paddle is set to a speed of 25-35rpm and the biaxial dispersion disk is set to a speed of 2000-3000rpm, and stirring is carried out for 150-240min; the third time, the twist paddle is set to a speed of 25-35rpm and the biaxial dispersion disk is set to a speed of 2000-3000rpm, and stirring is carried out for 30-60min. Vacuum -90~-95kpa defoaming treatment is performed to obtain CMC glue. Note that stirring may cause CMC to splash and adhere to the tank wall. Scrape off the CMC on the tank wall and put it back into water and stir to fully disperse it.

[0043] After the stirring is completed, a twin-screw mixer is used to prepare the mixture. First, CMC glue is added to the first feeding port of the twin-screw mixer, and the speed is set to 10-100rpm for rotation. Then, an appropriate amount of safety solute is added to the second feeding port, the speed is set to 10-100rpm, and the high-speed speed of the sand mill in the twin screw can be set to 1000-3000rpm. Next, polyacrylonitrile adhesive is added to the third feeding port, the speed is set to 10-100rpm, and the high-speed speed of the sand mill in the twin screw can be set to 1000-3000rpm. After stirring evenly, the above mixture is squeezed into a vacuum defoaming tank (not shown in the figure) for defoaming treatment to obtain the safety layer slurry.

[0044] The vacuum defoaming tank can be connected to the coating die head with the discharge pipe to complete direct and continuous discharge. The continuous twin-screw stirring discharge can control the discharge amount and ensure the stability of the safety layer slurry weight. The material ratio, stirring speed and system can be improved according to the discharge viscosity. The stirring parameters used in the above process are only the preferred solution, as long as the safety layer slurry is evenly dispersed, the viscosity is controlled within the range of 50-200CP, and the solid content is within the range of 3-10%.

[0045] The present invention controls the solid content of the safety layer slurry within the range of 3-10%. Such a small solid content can make the thickness of the safety layer thinner after drying, and the safety layer slurry extruded during coating is thicker, so that more slurry is extruded through the die head during extrusion coating, which is conducive to maintaining the pressure stability of the extrusion coating die head, making the safety layer thinner and the output amount more stable. The viscosity of the safety layer slurry is controlled at 50CP-200CP. If the viscosity is too low, the slurry is prone to overflow, which affects the uniformity of coating on the pole piece; if the slurry viscosity is increased, it is often necessary to increase the proportion of polyacrylonitrile adhesive. Too much proportion of polyacrylonitrile adhesive will increase the internal resistance of the battery and affect the battery performance. Therefore, the solid content and viscosity of the safety layer slurry of the present invention are conducive to the preparation of a pole piece coating that is both thin and safe, and will not affect the battery performance.

[0046] After the slurry is prepared, it is stored in a buffer and then enters the coating stage. In the coating stage, the slurry is subjected to extrusion force and is coated on the foil 3 through the extrusion coating die head. The coating of the present invention uses a combination of a multi-layer extrusion die head 2 and a single-layer extrusion die head 1 for coating. Figure 8 and Fig. 9 As shown, the arrow indicates the direction of the foil 3 unwinding, the multi-layer extrusion die 2 can coat multiple layers of active substances at the same time, and the single-layer extrusion die 1 is used to coat the safety layer. When the foil 3 is unrolled to the multi-layer extrusion die 2, the extruder extrude the slurry so that the active substance slurry is sprayed from the multi-layer die outlet to the foil 3, and then the safety layer slurry is sprayed from the single-layer die to cover the active substance layer.

[0047] In order to avoid the problem of increased battery internal resistance caused by the coating, when the active material layer slurry is coated, the active bottom layer that is bonded to the foil 3 uses a graphite material with a relatively small proportion of silicon-carbon doping and a higher gram capacity; the active upper layer uses a graphite material with a relatively large proportion of silicon-carbon doping, a lower gram capacity, but with fast charging performance. This can balance the gram capacity of the entire battery, avoid excessive silicon and carbon in the active bottom layer, which causes excessive rebound of the pole piece and insufficient adhesion between the coating and the pole piece, and avoid a large difference in resistance between the active upper layer and the safety layer. Using fast-charging materials as the active material layer can reduce the DC internal resistance and improve the lithium ion embedding ability.

[0048] As shown, a gasket is embedded in the outlet of each layer of the die head. The thicker the gasket, the thicker the coating. The larger the gasket opening, the wider the coating width. In order to make the safety layer thinner and have better thickness stability, the thickness of the gasket at the outlet of the safety layer slurry is designed to be 0.1-0.3mm. If the gasket thickness is too large, the thickness of the coated safety layer will be large, affecting the performance of the electrode. If the gasket thickness is too small, the pumping pressure of the extruder will easily cause the gasket to deform and wear more, resulting in a shorter gasket service life. Therefore, a gasket with a thickness of 0.1-0.3mm is a reasonable setting.

[0049] After each layer of slurry is extruded, the active material layer slurry close to the foil 3 has a higher viscosity and is not easy to flow, while the upper safety layer slurry has a lower viscosity and better fluidity and is easy to expand laterally. Therefore, the present invention further designs the gasket size, and the opening width of the gasket at the outlet of the single-layer extrusion die 1 is 2-4mm smaller than the opening width of the gasket at the outlet of the multi-layer extrusion die 2, so that the safety layer slurry can complete the covering and protection of the lower layer slurry after expansion.

[0050] Since the viscosity of the safety layer slurry is relatively low, the present invention further designs the chamfer of the safety layer slurry outlet gasket in the opening direction to be smaller than that in the depth direction, so as to avoid excessive thinning of the slurry or slurry overflow, making the discharge of the safety layer slurry smoother and more continuous. Further preferred chamfer dimensions in the opening direction are 3*5mm, 3*4mm, 2*4mm or 2*5mm, and the above chamfered gaskets can be used to prepare a safety layer that meets the process requirements.

[0051] The present invention defines the die gap between the single-layer extrusion die 1 and the active material layer on the foil 3 as 100-300um. If the die gap is too small, the active material layer slurry is still in a wet state and has a certain fluidity when the safety layer slurry is applied, and it is easily impacted by the kinetic energy of the safety layer slurry spraying, resulting in scraping, which affects the uniformity of the active material layer; if the die gap is too large, the safety layer slurry is too dispersed after spraying, and the coating may be missed. Therefore, the die gap within the above range can make the safety layer slurry fully cover the surface of the active material layer. In addition, the installation position of the single-layer extrusion die 1 is preferably arranged so that its spraying direction and the unwinding direction of the foil 3 are arranged at an acute angle of 30°-60° to reduce the impact of the spraying and prevent scraping. If the installation angle is greater than 60°, the safety layer slurry may overflow, and the density after coating may be unstable; if the installation angle is less than 30°, the angle of the paired active material layer slurry may be large, resulting in insufficient stability of the surface density of the active material layer slurry.

[0052] After coating, the slurry can be baked to evaporate the solvent, and the solid material can be bonded to the foil 3 to form the electrode. Since the solid content of the surface coating is reduced, the front oven should be set to low wind speed and high temperature for baking when baking in the oven. While ensuring that the solvent is baked out, the wind frequency should be avoided to prevent the electrode from shaking and causing a large deviation in the thickness of the surface coating. High wind frequency and high temperature are used for baking in the middle, and low wind frequency and low temperature are used when shipping out of the oven to avoid excessive deviation between the temperature of the electrode out of the oven and the ambient temperature, which may cause the electrode to dry and crack.

[0053] The drying may specifically include the following steps: in the first stage, the temperature is set at 70-85°C and the wind frequency is 10-20Hz for baking; in the second stage, the temperature is set at 70-85°C and the wind frequency is 20-40Hz for baking; in the third stage, the temperature is set at 55-70°C and the wind frequency is 10-20Hz for baking.

[0054] The invention prepares the safety layer slurry by twin-screw stirring, controls the solid content and viscosity of the safety layer slurry, and reasonably designs the gasket and coating parameters, so that the thickness of the coated safety layer is 3-6um, the flatness is within the range of ±1um, and the surface density is 3-6g / ㎡.

[0055] The present invention also proposes a battery negative electrode sheet prepared by the above-mentioned method of coating the battery negative electrode sheet safety layer slurry. The battery negative electrode sheet of the present invention has a thinner safety layer with good safety performance without affecting the energy density.

[0056] The specific implementation scheme of the present invention is described in detail below.

[0057] Example 1

[0058] Preparation of safety layer slurry: using 22.5 kg of carboxymethyl cellulose binder with a solid content of 0.5%, 3.75 kg of polyacrylonitrile binder with a solid content of 6%, and 7.163 kg of boehmite baking speed.

[0059] Preparation process: Preparation of CMC glue: Add pure water to the glue tank, then add carboxymethyl cellulose binder powder, stir slowly after adding, and sink the powder into the pure water. The glue is stirred in three steps: the first step is to set the twist paddle at a low speed of 15rpm, and the stirring time is 10min; the second step is to set the twist paddle at a low speed of 20rpm, the double-axis dispersion disk at a high speed of 1500rpm, and the stirring time is 30min; the third step is to set the twist paddle at a low speed of 30rpm, the double-axis dispersion disk at a high speed of 2000rpm, the stirring time is 180min, and vacuum-95kpa defoaming treatment is performed to obtain CMC glue. CMC glue is prepared using a 100L glue tank, and the glue produced by this glue tank is used in the later preparation of surface coating slurry.

[0060] Twin-screw stirring: first add CMC glue to the twin-screw feed port, and set the screw pump to rotate at 100rpm, then add boehmite at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2000rpm, continue to add polyacrylonitrile adhesive at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, continue to add pure water to adjust the slurry solid content to 7.54%, the viscosity to 179CP, set the speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, and finally put it into the vacuum defoaming tank for vacuum degassing after the stirring is completed. The vacuum degassing tank is connected to the coating tank to continuously transfer the slurry to the coating tank to complete continuous discharging.

[0061] Preparation of active material layer slurry: Select 2 different types of graphite materials, of which the upper graphite material is a fast-filling graphite material, and the bottom graphite material is a functional graphite material, wherein the fast-filling graphite material: the functional graphite material = 25:75, and the graphite material as the main powder accounts for 95.64% in the system, and the upper and bottom layers of the main graphite powder: polyacrylonitrile binder: CMC: carbon nanotubes: styrene-butadiene rubber binder = 95.64:2:0.5:0.8:0.06:1, wherein the weight of each substance added is calculated according to the weight of the above system, and is added separately. The system proportion refers to the solute proportion, the pure solid substance is graphite material and conductive carbon black, and the solid content of the polyacrylonitrile binder in the remaining materials is 6%, the solid content of the carbon nanotubes is 5%, and the solid content of the styrene-butadiene rubber binder is 40%. In order to prevent the problem of cracking of the negative electrode during baking, 1% of the weight of the graphite main powder is added as N-methylpyrrolidone solvent to prevent the cracking of the pole piece. The solid content of the active material layer slurry is 52% and the viscosity is 3500CP.

[0062] Coating: The active material layer is coated using a double-layer coating die head, which is divided into a bottom layer and an upper layer. The bottom layer gasket opening width is 267mm, the chamfer at the gasket opening direction is 2*3mm, and the gasket thickness is 0.7mm; the upper layer gasket opening width is 268mm, the chamfer at the gasket opening direction is 2*2mm, and the gasket thickness is 0.7mm. The gap between the multi-layer coating die head and the foil is 120um; the coating pump speed is 30rpm.

[0063] The safety layer slurry is coated with a single-layer coating die. The opening width of the single-layer coating die gasket is 265mm, the chamfer at the gasket opening direction is 3*5mm, the gasket thickness is 0.15mm, and the gap between the single-layer coating die and the active material layer is 55um; the coating pump speed is 140rpm.

[0064] Baking: The total length of the oven is 15m, and the length of one section is 3m. There are a total of 5 ovens connected in series, which can carry out three stages of baking. The baking speed is 10m / min. The first stage of baking uses the first and second ovens. The temperature of the first oven is set to 78°C and the wind frequency is 15Hz. The temperature of the second oven is 83°C and the wind frequency is 15Hz. The second stage of baking uses the third and fourth ovens. The temperature of the third oven is set to 78°C and the wind frequency is 25Hz. The temperature of the fourth oven is set to 70°C and the wind frequency is 25Hz. The third stage of baking uses the fifth oven. The temperature of the fifth oven is set to 63°C and the wind frequency is 10Hz. The SEM image of the cross-section of the safety layer of this embodiment is shown in the figure. Figure 2 As shown, the SEM image of the safety layer surface is as follows Fig.10 shown.

[0065] Example 2

[0066] Preparation of safety layer slurry: using 22.5 kg of carboxymethyl cellulose binder with a solid content of 0.5%, 3.75 kg of polyacrylonitrile binder with a solid content of 6%, and 7.163 kg of boehmite baking speed.

[0067] Preparation process: Preparation of CMC glue: Add pure water to the glue tank, then add carboxymethyl cellulose binder powder, stir slowly after adding, and sink the powder into the pure water. The glue is stirred in three steps: the first step is to set the twist paddle at a low speed of 15rpm, and the stirring time is 10min; the second step is to set the twist paddle at a low speed of 20rpm, the double-axis dispersion disk at a high speed of 1500rpm, and the stirring time is 30min; the third step is to set the twist paddle at a low speed of 30rpm, the double-axis dispersion disk at a high speed of 2000rpm, and the stirring time is 180min, and vacuum-95kpa defoaming treatment is performed to obtain CMC glue. CMC glue is prepared using a 100L glue tank, and the glue produced by this glue tank is used in the later preparation of surface coating slurry.

[0068] Twin-screw stirring: first add CMC glue to the twin-screw feed port, and set the screw pump to rotate at 100rpm, then add boehmite at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2000rpm, continue to add polyacrylonitrile adhesive at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, continue to add pure water to adjust the slurry solid content to 7.54%, the viscosity to 179CP, set the speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, and finally put it into the vacuum defoaming tank for vacuum degassing after the stirring is completed. The vacuum degassing tank is connected to the coating tank to continuously transfer the slurry to the coating tank to complete continuous discharging.

[0069] Preparation of active material layer slurry: Select 2 different types of graphite materials, of which the upper graphite material is a fast-filling graphite material, and the bottom graphite material is a functional graphite material, wherein the fast-filling graphite material: the functional graphite material = 25:75, and the graphite material as the main powder accounts for 95.64% in the system, and the upper and bottom layers of the main graphite powder: polyacrylonitrile binder: CMC: carbon nanotubes: styrene-butadiene rubber binder = 95.64:2:0.5:0.8:0.06:1, wherein the weight of each substance added is calculated according to the weight of the above system, and is added separately. The system proportion refers to the solute proportion, the pure solid substance is graphite material and conductive carbon black, and the solid content of the polyacrylonitrile binder in the remaining materials is 6%, the solid content of the carbon nanotubes is 5%, and the solid content of the styrene-butadiene rubber binder is 40%. In order to prevent the problem of cracking of the negative electrode during baking, 1% of the weight of the graphite main powder is added as N-methylpyrrolidone solvent to prevent the cracking of the pole piece. The solid content of the active material layer slurry is 52% and the viscosity is 3500CP.

[0070] Coating: The active material layer is coated using a double-layer coating die head, which is divided into a bottom layer and an upper layer. The bottom layer gasket opening width is 267mm, the chamfer at the gasket opening direction is 2*3mm, and the gasket thickness is 0.7mm; the upper layer gasket opening width is 268mm, the chamfer at the gasket opening direction is 2*2mm, and the gasket thickness is 0.7mm. The gap between the multi-layer coating die head and the foil is 120um; the coating pump speed is 30rpm.

[0071] The safety layer slurry is coated with a single-layer coating die. The opening width of the single-layer coating die gasket is 265mm, the chamfer at the gasket opening direction is 3*5mm, the gasket thickness is 0.15mm, and the gap between the single-layer coating die and the active material layer is 100um; the coating pump speed is 140rpm.

[0072] Baking: The total length of the oven is 15m, and the length of one section is 3m. There are a total of 5 ovens connected in series, which can carry out three stages of baking. The baking speed is 10m / min. The first stage of baking uses the first and second ovens. The temperature of the first oven is set to 78°C and the wind frequency is 15Hz. The temperature of the second oven is 83°C and the wind frequency is 15Hz. The second stage of baking uses the third and fourth ovens. The temperature of the third oven is set to 78°C and the wind frequency is 25Hz. The temperature of the fourth oven is set to 70°C and the wind frequency is 25Hz. The third stage of baking uses the fifth oven. The temperature of the fifth oven is set to 63°C and the wind frequency is 10Hz. The SEM image of the cross-section of the safety layer of this embodiment is shown in the figure. Figure 3 shown.

[0073] Example 3

[0074] Preparation of safety layer slurry: using 22.5 kg of carboxymethyl cellulose binder with a solid content of 0.5%, 3.75 kg of polyacrylonitrile binder with a solid content of 6%, and 7.163 kg of boehmite baking speed.

[0075] Preparation process: Preparation of CMC glue: Add pure water to the glue tank, then add carboxymethyl cellulose binder powder, stir slowly after adding, and sink the powder into the pure water. The glue is stirred in three steps: the first step is to set the twist paddle at a low speed of 15rpm, and the stirring time is 10min; the second step is to set the twist paddle at a low speed of 20rpm, the double-axis dispersion disk at a high speed of 1500rpm, and the stirring time is 30min; the third step is to set the twist paddle at a low speed of 30rpm, the double-axis dispersion disk at a high speed of 2000rpm, and the stirring time is 180min, and vacuum-95kpa defoaming treatment is performed to obtain CMC glue. CMC glue is prepared using a 100L glue tank, and the glue produced by this glue tank is used in the later preparation of surface coating slurry.

[0076] Twin-screw stirring: first add CMC glue to the twin-screw feed port, and set the screw pump to 100rpm for rotation, then add boehmite at the next feeding port, set the screw pump speed to 100rpm, set the sand mill high-speed speed in the twin screw to 2000rpm, continue to add polyacrylonitrile adhesive at the next feeding port, set the screw pump speed to 100rpm, set the sand mill high-speed speed in the twin screw to 2500rpm, continue to add pure water to adjust the slurry solid content to 10%, the viscosity to 192CP, set the screw pump speed to 100rpm, set the sand mill high-speed speed in the twin screw to 2500rpm, and finally put it into the vacuum defoaming tank for vacuum degassing after the stirring is completed. The vacuum degassing tank is connected to the coating tank to continuously transfer the slurry to the coating tank to complete continuous discharging.

[0077] Preparation of active material layer slurry: Select 2 different types of graphite materials, of which the upper graphite material is a fast-filling graphite material, and the bottom graphite material is a functional graphite material, wherein the fast-filling graphite material: the functional graphite material = 25:75, and the graphite material as the main powder accounts for 95.64% in the system, and the upper and bottom layers of the main graphite powder: polyacrylonitrile binder: CMC: carbon nanotubes: styrene-butadiene rubber binder = 95.64:2:0.5:0.8:0.06:1, wherein the weight of each substance added is calculated according to the weight of the above system, and is added separately. The system proportion refers to the solute proportion, the pure solid substance is graphite material and conductive carbon black, and the solid content of the polyacrylonitrile binder in the remaining materials is 6%, the solid content of the carbon nanotubes is 5%, and the solid content of the styrene-butadiene rubber binder is 40%. In order to prevent the problem of cracking of the negative electrode during baking, 1% of the weight of the graphite main powder is added as N-methylpyrrolidone solvent to prevent the cracking of the pole piece. The solid content of the active material layer slurry is 52% and the viscosity is 3500CP.

[0078] Coating: The active material layer is coated using a double-layer coating die head, which is divided into a bottom layer and an upper layer. The bottom layer gasket opening width is 267mm, the chamfer at the gasket opening direction is 2*3mm, and the gasket thickness is 0.7mm; the upper layer gasket opening width is 268mm, the chamfer at the gasket opening direction is 2*2mm, and the gasket thickness is 0.7mm. The gap between the multi-layer coating die head and the foil is 120um; the coating pump speed is 30rpm.

[0079] The safety layer slurry is coated with a single-layer coating die. The opening width of the single-layer coating die gasket is 265mm, the chamfer at the gasket opening direction is 3*5mm, the gasket thickness is 0.15mm, and the gap between the single-layer coating die and the active material layer is 55um; the coating pump speed is 140rpm.

[0080] Baking: The total length of the oven is 15m, and the length of one section is 3m. There are a total of 5 ovens connected in series, which can carry out three stages of baking. The baking speed is 10m / min. The first stage of baking uses the first and second ovens. The temperature of the first oven is set to 75℃, and the wind frequency is 15Hz. The temperature of the second oven is 80℃, and the wind frequency is 15Hz. The second stage of baking uses the third and fourth ovens. The temperature of the third oven is set to 75℃, and the wind frequency is 25Hz. The temperature of the fourth oven is set to 70℃, and the wind frequency is 25Hz. The third stage of baking uses the fifth oven. The temperature of the fifth oven is set to 60℃, and the wind frequency is 10Hz. The SEM image of the cross-section of the safety layer of this embodiment is shown in the figure. Figure 4 shown.

[0081] Example 4

[0082] Preparation of safety layer slurry: using 22.5 kg of carboxymethyl cellulose binder with a solid content of 0.5%, 3.75 kg of polyacrylonitrile binder with a solid content of 6%, and 7.163 kg of boehmite baking speed.

[0083] Preparation process: Preparation of CMC glue: Add pure water to the glue tank, then add carboxymethyl cellulose binder powder, stir slowly after adding, and sink the powder into the pure water. The glue is stirred in three steps: the first step is to set the twist paddle at a low speed of 15rpm, and the stirring time is 10min; the second step is to set the twist paddle at a low speed of 20rpm, the double-axis dispersion disk at a high speed of 1500rpm, and the stirring time is 30min; the third step is to set the twist paddle at a low speed of 30rpm, the double-axis dispersion disk at a high speed of 2000rpm, and the stirring time is 180min, and vacuum-95kpa defoaming treatment is performed to obtain CMC glue. CMC glue is prepared using a 100L glue tank, and the glue produced by this glue tank is used in the later preparation of surface coating slurry.

[0084] Twin-screw stirring: first add CMC glue to the twin-screw feed port, and set the screw pump to 100rpm for rotation, then add boehmite at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2000rpm, continue to add polyacrylonitrile adhesive at the next feeding port, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, continue to add pure water to adjust the slurry solid content to 7.54%, the viscosity to 179CP, set the screw pump speed to 100rpm, set the high-speed speed of the sand mill in the twin screw to 2500rpm, and finally put it into the vacuum defoaming tank for vacuum degassing after the stirring is completed. The vacuum degassing tank is connected to the coating tank to continuously transfer the slurry to the coating tank to complete continuous discharging.

[0085] Preparation of active material layer slurry: Select 2 different types of graphite materials, of which the upper graphite material is a fast-filling graphite material, and the bottom graphite material is a functional graphite material, wherein the fast-filling graphite material: the functional graphite material = 25:75, and the graphite material as the main powder accounts for 95.64% in the system, and the upper and bottom layers of the main graphite powder: polyacrylonitrile binder: CMC: carbon nanotubes: styrene-butadiene rubber binder = 95.64:2:0.5:0.8:0.06:1, wherein the weight of each substance added is calculated according to the weight of the above system, and is added separately. The system proportion refers to the solute proportion, the pure solid substance is graphite material and conductive carbon black, and the solid content of the polyacrylonitrile binder in the remaining materials is 6%, the solid content of the carbon nanotubes is 5%, and the solid content of the styrene-butadiene rubber binder is 40%. In order to prevent the problem of cracking of the negative electrode during baking, 1% of the weight of the graphite main powder is added as N-methylpyrrolidone solvent to prevent the cracking of the pole piece. The solid content of the active material layer slurry is 52% and the viscosity is 3500CP.

[0086] Coating: The active material layer is coated using a double-layer coating die head, which is divided into a bottom layer and an upper layer. The bottom layer gasket opening width is 267mm, the chamfer at the gasket opening direction is 2*3mm, and the gasket thickness is 0.7mm; the upper layer gasket opening width is 268mm, the chamfer at the gasket opening direction is 2*2mm, and the gasket thickness is 0.7mm. The gap between the multi-layer coating die head and the foil is 120um; the coating pump speed is 30rpm.

[0087] The safety layer slurry is coated with a single-layer coating die. The opening width of the single-layer coating die gasket is 265mm, the chamfer at the gasket opening direction is 3*5mm, the gasket thickness is 0.10mm, and the gap between the single-layer coating die and the active material layer is 55um; the coating pump speed is 140rpm.

[0088] Baking: The total length of the oven is 15m, and the length of one section is 3m. There are a total of 5 ovens connected in series, which can carry out three stages of baking. The baking speed is 10m / min. The first stage of baking uses the first and second ovens. The temperature of the first oven is set to 78°C and the wind frequency is 15Hz. The temperature of the second oven is 83°C and the wind frequency is 15Hz. The second stage of baking uses the third and fourth ovens. The temperature of the third oven is set to 78°C and the wind frequency is 25Hz. The temperature of the fourth oven is set to 70°C and the wind frequency is 25Hz. The third stage of baking uses the fifth oven. The temperature of the fifth oven is set to 63°C and the wind frequency is 10Hz. The SEM image of the cross-section of the safety layer of this embodiment is shown in the figure. Figure 5 shown.

[0089] Comparative Example 1

[0090] The solid content of the safety layer slurry solution is 13.5%, and the viscosity is 340CP. The solid content is relatively high. The coating and baking temperature is 2°C lower than that of Example 1. The other preparation parameters, coating method and baking method are the same as those of Example 1. The cross-sectional SEM image of the safety layer of this comparative example is shown in FIG. Figure 6 shown.

[0091] Comparative Example 2

[0092] The thickness of the safety layer slurry is 0.4 mm, and the other preparation parameters, slurry solid content, coating method and baking method are the same as those in Example 1. The cross-sectional SEM image of the safety layer of this comparative example is shown in FIG. Figure 7 shown.

[0093] Comparative Example 3

[0094] The safety layer slurry and active material layer slurry of Example 1 were used. During coating, the distance between the coating die head of the safety layer slurry and the active material layer was 120 μm. The other preparation parameters, coating method and baking method were the same as those of Example 1. The cross-sectional SEM image of the safety layer of this comparative example is shown in FIG. Figure 8 shown.

[0095] Comparative Example 4

[0096] The solid content of the safety layer slurry solution is 2.5%, the viscosity is 38CP, the solid content is relatively high, and the coating and baking temperature is 2°C higher than that of Example 1. The other preparation parameters, coating method and baking method are the same as those of Example 1. The cross-sectional SEM image of the safety layer of this comparative example is shown in FIG. Fig. 9 As shown, the SEM image of the safety layer surface is as follows Fig.11 shown.

[0097] The present invention carries out safety layer coating according to the above 8 methods, and the main coating parameters are summarized as shown in Table 1; the safety layer data of each embodiment and comparative example are measured, as shown in Table 2. Among them, the debugging parameters of embodiment 1 are the best, the average thickness of embodiment 1 is 3.2μm, and the thickness fluctuation at each point is within the range of the average value ±1μm. Figure 2 As shown, the SEM image of the cross section of the safety layer of Example 1 shows that the coating thickness is about 3 um, the safety layer and the active material layer can be clearly distinguished, and the coating of the safety layer is very uniform.

[0098] Table 1

[0099] Speed ​​m / min Pump speed rpm Die head gap um Solid content% Viscosity CP Comparative Example 1 10 140 55 13.50% 340 Comparative Example 2 10 140 55 7.54% 179 Comparative Example 3 10 140 120 7.54% 179 Comparative Example 4 10 140 55 2.50% 38 Example 1 10 140 55 7.54% 179 Example 2 10 140 100 7.54% 179 Example 3 10 140 55 10.00% 192 Example 4 10 140 55 7.54% 179

[0100] Table 2

[0101]

[0102] observe Fig.10 and Fig.11 , compare the surface morphology of safety coatings of different thicknesses, and observe Fig.10 In the surface SEM image, only the safety solute material can be seen, and the active material material cannot be seen through the safety layer, which shows that the safety layer of Example 1 completely covers the surface of the active material layer and has good safety performance. Fig.11 From the surface SEM image, the graphite material of the active material layer can be seen through the safety layer, indicating that the safety layer of Comparative Example 4 cannot play a safety role.

[0103] It can be seen from Table 2 that the safety layer of each embodiment of the present invention is better than the comparative example in terms of performance indicators such as coating thickness and coating width. The coating method of the present invention can make the electrode have a thinner thickness and good safety without affecting the energy density.

[0104] The above embodiments and comparative examples were subjected to a needle puncture test, using a steel needle with a diameter of 5 mm and a length of 25 mm at a puncture speed of 25 mm / s, to test the safety performance and comparative energy density loss of the prepared pole pieces. The test results are shown in Table 3 below:

[0105] Table 3

[0106] plan Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Fire No fire No fire No fire No fire No fire No fire No fire Fire Maximum temperature: ℃ 84 87 76 89 73 68 85 358 Acupuncture results pass pass pass pass pass pass pass Not passed Energy density loss % 0.81% 0.83% 0.95% 0.74% 1.82% 1.93% 1.12% 0.65%

[0107] Table 3 shows that: Examples 1-4 and Comparative Examples 1-3 can pass the needle puncture test, and no thermal diffusion problem occurs, which has good safety performance; however, the energy density loss of each example is significantly less than that of Comparative Examples 1-3, indicating that the safety layer coated by this method can make the pole piece have a thinner thickness and good safety without affecting the energy density. Compared with Examples 1-4 and Comparative Example 4, although the energy density loss of Example 1-4 is slightly greater than that of Comparative Example 4, Comparative Example 4 cannot pass the needle puncture test and is not safe enough, while the energy density loss of Example 1-4 is acceptable.

[0108] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0109] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A method for coating a safety layer slurry of a battery negative electrode sheet, comprising preparing the safety layer slurry, extrusion coating and drying, Features: The safety layer slurry is prepared by mixing carboxymethyl cellulose binder and pure water to form CMC glue solution, and the CMC glue solution is mixed and stirred evenly with safety solute and polyacrylonitrile binder in a twin-screw mixer. The solid content of the safety layer slurry solution is 3-10%, and the viscosity is 50-200CP; The extrusion coating is to coat the safety layer slurry on the basis of the coating of the active material layer slurry, wherein the active material layer slurry is coated between the coated foil and the safety layer slurry, during coating, the distance between the coating die head of the safety layer slurry and the active material layer is 50-100 μm, and the thickness of the safety layer slurry outlet gasket is 0.1-0.3 mm; The safety layer slurry preparation comprises the following steps: preparing CMC glue solution: adding carboxymethyl cellulose binder and pure water into a glue tank, using a PD mixer to stir for multiple times, setting the twist paddle to stir at a low speed of 15-30rpm for 10-45min for the first time; setting the twist paddle at a speed of 20-35rpm and the biaxial dispersion disk at a speed of 1000-3000rpm for the second time, stirring for 30-60min at the same time; setting the twist paddle at a speed of 25-35rpm and the biaxial dispersion disk at a speed of 2000-3000rpm for the third time, stirring for 30-60min at the same time; setting the twist paddle at a speed of 25-35rpm and the biaxial dispersion disk at a speed of 2000-3000rpm for the third time, stirring for 30-60min at the same time; setting the twist paddle at a speed of 25-35rpm and the biaxial dispersion disk at a speed of 2000-3000rpm for the third time, stirring for 30-60min at the same time; setting the twist paddle at a speed of 20 ... rpm, stirring for 150-240min, and controlling the vacuum within the range of -90---99kPa to obtain the CMC glue solution; twin-screw stirring: adding the CMC glue solution to the first feeding port of the twin-screw mixer, rotating at a speed of 10-100rpm, adding the safety solute and polyacrylonitrile adhesive to the second and third feeding ports respectively, rotating at a speed of 10-100rpm, and high-speed sand milling and stirring at a speed of 1000-3000rpm; obtaining the safety layer slurry after vacuum defoaming; The safety layer thickness of the prepared battery negative electrode sheet is 3-6 μm, the flatness is within the range of ±1 μm, and the surface density is 3-6 g / ㎡.

2. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 1, Features: The raw materials for preparing the safety layer slurry include carboxymethyl cellulose binder, polyacrylonitrile binder and effective ingredients in the safety solute in a weight ratio of (0.5-2):(1-5):(87-97), and the safety solute includes at least one of boehmite and silicon dioxide.

3. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 1, Features: The effective ingredients in the silicon-carbon material, conductive carbon black, polyacrylonitrile binder, carboxymethyl cellulose binder and styrene-butadiene rubber binder in the raw materials for preparing the active material layer slurry are in a weight ratio of (90-98): (0.5-5): (0.5-3): (0.5-2): (0.5-2.5).

4. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 3, Features: The silicon-carbon material includes graphite and silicon-oxygen material, wherein the silicon-oxygen material accounts for 3-30% of the silicon-carbon material.

5. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 1, Features: The opening width of the safety layer slurry outlet gasket is 2-4 mm smaller than the opening width of the active material layer slurry outlet gasket.

6. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 1, Features: The chamfer of the safety layer slurry outlet gasket in the opening direction is smaller than that in the depth direction.

7. The method for coating the safety layer slurry of the battery negative electrode sheet according to claim 5, Features: The chamfer of the safety layer slurry outlet gasket in the opening direction is 3*5mm, 3*4mm, 2*4mm or 2*5mm.

8. The method for coating the battery negative electrode safety layer slurry according to any one of claims 1 to 7, Features: The drying comprises the following steps: in the first stage, the temperature is set at 70-85°C and the wind frequency is 10-20Hz for baking; in the second stage, the temperature is set at 70-85°C and the wind frequency is 20-40Hz for baking; in the third stage, the temperature is set at 55-70°C and the wind frequency is 10-20Hz for baking.

9. A battery negative electrode sheet prepared by the method for coating a battery negative electrode sheet safety layer slurry according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of negative electrode slurry without glue solution, obtained negative electrode slurry and application

    CN111725508A

  • Lithium ion secondary battery pole piece and lithium ion secondary battery

    CN111725511A