A biomass-based SnO y @C / SiO x Composite material and its preparation method and application
The preparation of biomass-based SnOy@C/SiOx composite materials has solved the problems of cycle performance and environmental pollution of lithium-ion battery anode materials, and realized the industrial application of high-capacity, low-cost lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202210837649.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-07-15
AI Technical Summary
Existing lithium-ion battery anode materials such as graphite, silicon, and tin oxide have shortcomings in terms of cycle performance, conductivity, and volume expansion, which limit their commercial application. Furthermore, existing preparation methods suffer from environmental pollution and high costs.
A biomass-based SnOy@C/SiOx composite material was prepared by using a carbothermic reduction and disproportionation reaction between tin compounds and carbon and silicon in biomass to construct an organic whole of SnOy/C/SiOx, which alleviates volume expansion and improves conductivity and cycle stability.
The prepared material exhibits excellent cycle stability and high capacity at high current density, is environmentally friendly and low in cost, and is suitable for high-rate, high-capacity power battery electrode materials.
Smart Images

Figure CN115275133B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a biomass-based SnO y @C / SiO x Composite materials and their preparation methods and applications. Background Art
[0002] Lithium-ion batteries are widely used in mobile phones, power tools, hybrid and electric vehicles due to their high cycle performance, environmental friendliness, high energy and power density, and are integrated into daily life. They have become a huge driving force for the development of clean energy storage devices. Currently, the commercial negative electrode of lithium batteries is mainly graphite material with a theoretical capacity of only 372mAh / g, which cannot meet the requirements of today's era for high energy storage, fast energy storage, and fast release, hindering the development of lithium-ion batteries.
[0003] Silicon has a theoretical capacity of up to 4200mAh / g, abundant storage resources, easy extraction, and low price. It is expected to become the king of negative electrodes in secondary batteries. However, due to its low first coulombic efficiency (first efficiency) and poor conductivity, it is very easy to expand / contract in volume during the lithium ion insertion / extraction process, causing the electrode to pulverize and fall off, and capacity decay, which in turn restricts its industrial application. Tin oxide has a theoretical capacity of 1494mAh / g, which is far better than commercial graphite, but its commercial application is also limited by the volume expansion effect and conductivity. However, its abundant reserves and low production cost also make it an ideal candidate material for negative electrodes in secondary batteries. Although the theoretical capacity of graphite is only 372mAh / g, it has become the most widely used commercial material due to its ultra-high cycle stability and excellent conductivity.
[0004] Biomass as a sustainable energy source has gradually attracted widespread attention, and its richness in silicon, carbon and other elements has triggered a wave of researchers to develop and utilize biomass energy, including purifying SiO2 to prepare high-toughness cement and special ceramics, preparing adsorbent carbon through zinc chloride pore formation, and preparing C / SiO2 through aluminothermic or magnesia thermal reactions. xNegative electrode materials, etc. However, the strong toxicity of zinc chloride has always been a concern for the public, and in the production process of aluminum / magnesium thermal reaction, the material needs to be treated with acid for secondary treatment to remove by-products, which causes great damage to the environment, and also causes a significant increase in production costs and a sharp consumption and waste of auxiliary raw materials. The Chinese invention patent with application publication number CN111009648B discloses a silicon-carbon composite material and a preparation method thereof (Yu Xiaoyuan, Chen Wenyan, Kuang Shaojie, Chen Yuancheng [P]); the Chinese invention patent with application publication number CN106450220B discloses a silicon-carbon composite material and a preparation method thereof (Han Jiantao [P]); the invention patent with application publication number CN113611843 A discloses a biomass-based porous silicon-carbon composite material and a preparation method thereof (Hou Jiao et al. [P]); the invention patent with application publication number CN 110867567 A discloses a preparation method and application of a highly safe biomass silicon synthesized SiOx@C material (Hu Pei et al. [P]), which all need to be pickled after carbonization treatment, causing pollution in production.
[0005] The Chinese invention patent with application publication number CN 113314702B discloses a carbon-silicon coated tin dioxide composite, its preparation method and its application as a negative electrode material for lithium-ion batteries. It first carbonizes biomass to obtain carbon, and then compounds the carbon with ionic liquid to obtain biocarbon; then, ball-mills pure silicon with nano-SnO2 and then compounds with biocarbon to obtain a carbon-silicon coated tin oxide material. The process is complicated, and the first coulombic efficiency and specific capacity of the obtained material are relatively low. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing SnO using silicon-containing biomass. y @C / SiO x The composite material and its preparation method and application give full play to the characteristics of biomass rich in silicon and carbon, and introduce tin compounds to reduce silicon dioxide in biomass, and then prepare the negative electrode material of lithium-ion battery. The preparation method is simple, safe, non-toxic and pollution-free. The prepared product has excellent performance and great market competitiveness. The capacity after 100 cycles at a current density of 2A / g is about 870.2mAh / g. Similarly, after the negative electrode is activated by a small current, the capacity can still be maintained at 523mAh / g after 7700 cycles at an ultra-large current of 10A / g.
[0007] The technical solution adopted by the present invention is mainly:
[0008] The present invention provides a biomass-based SnO y @C / SiO x A method for preparing a composite material (0≤[x,y]<2) comprising the following steps:
[0009] (1) Pretreatment and crushing of silicon-containing biomass;
[0010] (2) mixing the tin compound with the biomass raw material obtained in step (1) in a certain ratio;
[0011] (3) subjecting the product obtained in step (2) to carbonization treatment in an inert atmosphere and maintaining the temperature for a period of time;
[0012] (4) The product of step (3) is crushed and sieved to obtain the biomass-based SnO y @C / SiO x Composite materials.
[0013] Furthermore, in the above technical solution, in step (1), clean biomass raw materials with a mesh size of 60-350 are obtained through pretreatment and crushing.
[0014] Furthermore, in the above technical solution, the silicon-containing biomass is rich in silicon, including one or a mixture of two or more of rice straw, rice husk, straw, bamboo leaves, wheat husk, reed, sedge, sedge, and peanut shell.
[0015] Furthermore, in the above technical scheme, the tin compound includes one or a mixture of two or more of SnO2, Sn(NO3)2, Sn(NO3)4, C2H6O6S2Sn, SnC2O4, K2SnO2, K2SnO3, Sn(OH)2, Sn(OH)4, SnS, SnS2, Sn, and SnO.
[0016] Furthermore, in the above technical solution, the mixing in a certain proportion in step (2) is such that the tin compound after mixing accounts for 10-80wt% of the total mass, preferably 20-60wt%.
[0017] Furthermore, in the above technical solution, the temperature range of the carbonization treatment is 450-1200°C, preferably: 550-850°C; the heating rate is 1-20°C / min, and the insulation time is 0.5-6h, preferably: the heating rate is 5-10°C / min, and the insulation time is 1-4h; the inert atmosphere includes argon, nitrogen, helium or Ar / N2 mixed gas.
[0018] The present invention also provides a biomass-based SnO y @C / SiO x (0≤[x,y]<2) composite material, the composite material is composed of SnO y and C / SiO x Composition, SiO x Randomly dispersed in the biomass carbon skeleton, while SnO yThe particles are in the form of spheres, flowers, flakes, lines, strips, filaments or dendrites and are embedded in the surface and gaps of the biomass carbon skeleton.
[0019] The present invention also provides biomass-based SnO prepared by the above preparation method y @C / SiO x (0≤[x,y]<2) composite material or the biomass-based SnO y @C / SiO x (0≤[x,y]<2) Application of composite materials in negative electrode materials of lithium-ion batteries.
[0020] The present invention uses silicon-rich biomass as raw material. The basic preparation principle is to utilize the carbon thermal reduction reaction between tin compounds and carbon in the biomass matrix and the disproportionation reaction of tin compounds at high temperature to reduce the silicon dioxide in the biomass, thereby reducing low-oxygen silicide with high capacity advantage. Specifically, taking SnO2 as an example, the preparation process involves the following chemical reactions or disproportionation reactions, including:
[0021] SnO2(s)+C(s)=Sn(l)+CO2(g) (1)
[0022] 2SnO2(s)+C(s)=2SnO(s)+CO2(g) (2)
[0023] 2SnO(s)=Sn(l)+SnO2(s) (3)
[0024] SiO2+2SnO(g)=SiO x (s)+2SnO 2-0.5x (s) (4)
[0025] The desired biomass-based SnOy@C / SiOx composite material for lithium-ion battery anode can be prepared by carbonization pyrolysis of a mixture of silicon-rich biomass and tin compounds and a series of reactions.
[0026] The advantages and beneficial effects of the present invention are as follows:
[0027] (1) The natural structure of biomass waste not only constructs a C / SiO2 biomass carbon skeleton that is embedded in each other and serves as a template for each other, but also provides a basis for SnO y The mosaic provides convenience for constructing SnO y / C / SiO x The organic unified whole can effectively alleviate the volume expansion of tin and silicon during the cyclic charge and discharge process, prevent the electrode material from pulverizing and falling off from the current collector, and improve the cycle stability.
[0028] (2) SnO yAs a high energy storage material, it can not only play the role of metal properties to improve its initial efficiency and conductivity, but also undergo carbon thermal reduction reaction and disproportionation reaction during the thermal reduction process, thereby synergistically reducing the silicon in the biomass, giving full play to its silicon-rich properties to improve the reversible capacity of the material. When the material prepared by the scheme of the present invention is used as a negative electrode, the capacity after 100 cycles at a current density of 2A / g is about 870.2mAh / g. Similarly, after the negative electrode is activated by a small current, the capacity can still be maintained at 523mAh / g after 7700 cycles of an ultra-large current of 10A / g.
[0029] (3) Biomass is a renewable energy source and agricultural waste. Using it to prepare negative electrode materials for lithium secondary batteries can effectively solve the environmental problems caused by its incineration. At the same time, biomass is a renewable energy source with wide distribution, large reserves, low price, simple processing, and convenient industrial production. It can bring significant economic benefits to the manufacturing industry and increase farmers' income.
[0030] (4)SnO y The introduction of effectively improves the vibration, compaction and filling density of the material, so that it can be used to prepare high-rate and large-capacity power battery electrode materials.
[0031] (5) Compared with carbon thermal reduction of SiO2, the temperature requirement is high (reaching above 2000°C); although the reduction temperature of aluminothermic and magnesothermic reactions is greatly reduced, aluminum or magnesium elements are relatively introduced, and then aluminum salts or magnesium salts are formed, which need to be removed with acid in the later stage. The process is complicated, the cost is high, and it also causes damage to the environment. The scheme of the present invention is simple and easy to implement, does not use special equipment and devices, has low energy consumption, no waste of raw materials, does not introduce and does not produce toxic and harmful substances, reduces the input of resources in industrial production, realizes the efficient utilization of raw materials, and achieves the goals of low investment, low cost, high return and high value, which meets the requirements of green chemical industry.
[0032] (6) The present invention utilizes the complementary advantages of carbon, silicon and tin, and adopts a method combining simple physical mixing and inert atmosphere carbonization. The disproportionation reaction of tin and the carbon thermal reduction effect are used to synergistically reduce the silicon dioxide in biomass materials such as rice husks, thereby optimizing the first coulombic efficiency of the product. The material prepared by the present invention has the characteristics of high capacity, large rate, good conductivity, and excellent cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The SnO prepared in Example 1 of the present invention y @C / SiO x XRD patterns of the composite materials.
[0034] Figure 2 The SnO prepared in Example 1 of the present invention y @C / SiOx SEM images of the composite materials.
[0035] Figure 3 The SnO prepared in Example 1 of the present invention y @C / SiO x Cycling performance diagram of the composite material at a current density of 2 A / g.
[0036] Figure 4 The SnO prepared in Example 1 of the present invention y @C / SiO x Cycling performance diagram of the composite material at a current density of 10 A / g. DETAILED DESCRIPTION
[0037] In order to enable ordinary technicians in the field to more clearly understand the purpose, advantages and technical solutions of the present invention, the present invention is described in detail below in conjunction with embodiments. The embodiments are only used to illustrate the present invention and do not limit the scope of the present invention.
[0038] Example 1
[0039] A biomass-based SnO y @C / SiO x The preparation method of the composite material is as follows:
[0040] ① Wash, filter, dry and crush the rice husk containing silicon biomass, and sieve through 80 mesh to obtain clean rice husk powder raw material;
[0041] ② Add tin compound tin dioxide into the rice husk powder raw material at a ratio of 20wt% and mix them thoroughly and evenly;
[0042] ③Put the mixture in a heating furnace, heat it to 650℃ at a rate of 5℃ / min under the protection of inert atmosphere argon, calcine it for 2h, cool it naturally to room temperature, and obtain the required SnO after crushing and screening. y @C / SiO x (0≤[x,y]<2) Composite materials( Figure 1 SnO y @C / SiO x XRD pattern of the composite material).
[0043] The obtained SnO y @C / SiO x (0≤[x,y]<2) The composite material is composed of SnO y and C / SiO x Composition, SiO x Randomly dispersed in the biomass carbon skeleton, while SnO y The particles in the form of balls, flowers, flakes, lines, strips, filaments or dendrites are embedded in the surface and gaps of the biomass carbon skeleton ( Figure 2 ).
[0044] The obtained SnO y @C / SiO x The electrode prepared by the composite material (0≤[x,y]<2) can maintain a specific capacity of 870.2mAh / g after 100 cycles at a current density of 2A / g ( Figure 3 ), after low current activation, it can maintain a specific capacity of 523mAh / g after 7700 cycles at a current density of 10A / g, showing ultra-high cycle stability ( Figure 4 ).
[0045] Example 2
[0046] A biomass-based SnO y @C / SiO x The preparation method of the composite material is as follows:
[0047] ① Wash, filter, dry, and crush the sedge, and sieve through 60 meshes to obtain clean sedge powder raw material;
[0048] ② Add tin hydroxide of the tin compound into the sedge powder raw material at a ratio of 80%, and mix them thoroughly and evenly;
[0049] ③Put the mixture in a heating furnace, heat it to 450℃ at a rate of 10℃ / min under the protection of inert atmosphere nitrogen, calcine for 3h, cool it naturally to room temperature, and obtain the required SnO after crushing and screening. y @C / SiO x (0≤[x,y]<2) composite material.
[0050] Example 3
[0051] The bamboo leaves are washed, filtered, dried, crushed, and sieved through 200 meshes to obtain a clean bamboo leaf powder raw material; the tin compound tin oxalate is added to the bamboo leaf powder raw material at a ratio of 60wt% and mixed thoroughly and evenly; the mixture is placed in a heating furnace with an Ar / N2 mixed atmosphere, heated to 750°C at a rate of 2°C / min, calcined for 1.5h, cooled naturally to room temperature, crushed, and sieved to obtain the desired SnO y @C / SiO x (0≤[x,y]<2) composite material.
[0052] Example 4
[0053] The reeds are washed, filtered, dried, crushed, and sieved through 100 meshes to obtain clean reed powder raw materials; tin compound tin nitrate is added to the reed powder raw materials at a ratio of 40wt%, and the mixture is fully and evenly mixed; the mixture is placed in a heating furnace with N2 atmosphere, heated to 1000℃ at a rate of 20℃ / min, calcined for 1h, naturally cooled to room temperature, crushed, and sieved to obtain the required SnO y @C / SiO x (0≤[x,y]<2) composite material.
[0054] Example 5
[0055] Wash, filter, dry and crush the peanut shells, and sieve through 300 meshes to obtain clean peanut shell powder raw materials; add tin compound tin sulfide to the peanut shell powder raw materials at a ratio of 50wt%, and mix them thoroughly and evenly; place the mixture in a heating furnace with N2 atmosphere, heat it to 1200℃ at a rate of 15℃ / min, calcine it for 0.5h, cool it naturally to room temperature, crush it and sieve it to obtain the required SnO y @C / SiO x (0≤[x,y]<2) composite material.
[0056] Example 6: Preparation of negative electrode sheet
[0057] The SnO prepared in Example 1 y @C / SiO x The (0≤[x,y]<2) composite material is uniformly mixed with Super-P (conductive carbon black) and sodium alginate in a mass ratio of 7:2:1, coated on a copper foil, placed in a vacuum drying oven at 60°C for 12 hours, and rolled to obtain a negative electrode sheet for assembling a lithium-ion battery.
[0058] Table 1 shows the SnO prepared in Example 1. y @C / SiO x The (0≤[x,y]<2) composite material was made into a negative electrode. The capacity and capacity retention rate at different cycle numbers at a current density of 0.2A / g showed that the capacity retention rate was 59.97% after 90 cycles of charge and discharge, and the capacity was still maintained at a high 1100mAh g -1 The negative electrode is matched with the positive electrode made of lithium iron phosphate to assemble a lithium-ion battery LiFePO4||SnO y @C / SiO x , and its first Coulombic efficiency reached over 85%.
[0059] Table 1
[0060]
[0061] The various embodiments of the present invention described above can be freely combined, and the above embodiments are only partial embodiments. Those skilled in the art may make various changes and modifications based on the present invention. Therefore, any modification, equivalent replacement and improvement made within the scope of the principles and spirit of the present invention shall be within the protection scope of the present invention.
Claims
1. A biomass-based SnO y @C / SiO x Application of a composite material (0≤[x,y]<2) in a negative electrode material for a lithium-ion battery, characterized in that: Biomass-based SnO y @C / SiO x A method for preparing a composite material (0≤[x,y]<2) comprising the following steps: (1) Pretreatment and crushing of silicon-containing biomass; (2) mixing the tin compound with the biomass raw material obtained in step (1) in a certain ratio; (3) subjecting the product obtained in step (2) to carbonization treatment in an inert atmosphere and maintaining the temperature for a period of time; (4) The product of step (3) is crushed and sieved to obtain the biomass-based SnO y @C / SiO x Composite materials; The silicon-containing biomass is rich in silicon, and includes one or a mixture of two or more of rice straw, rice husk, corn stalk, bamboo leaf, wheat husk, reed, wheat, and peanut shell; The tin compound includes one or a mixture of two or more of SnO2, Sn(NO3)2, Sn(NO3)4, C2H6O6S2Sn, SnC2O4, K2SnO2, K2SnO3, Sn(OH)2, Sn(OH)4, SnS, SnS2, Sn, SnO; The mixing in a certain proportion in step (2) is such that the tin compound after mixing accounts for 10-80wt% of the total mass of the substance; The temperature range of the carbonization treatment is 550-850°C; the heating rate is 1-20°C / min, and the holding time is 0.5-6h; the inert atmosphere includes argon, nitrogen, helium or Ar / N2 mixed gas; The biomass-based SnO y @C / SiO x (0≤[x,y]<2) The composite material is composed of SnO y 、C / SiO x Composition, SiO x Randomly dispersed in the biomass carbon skeleton, while SnO y The particles are in the form of spheres, flowers, flakes, lines, strips, filaments or dendrites and are embedded in the surface and gaps of the biomass carbon skeleton.
2. The use according to claim 1, characterized in that: In step (1), clean biomass raw materials with a mesh size of 60-350 are obtained through pretreatment and crushing.