Lead sulfide quantum dot preparation method, near-infrared solar cell, photodetector
By using a vacuum heating method of lead sources, organic ligands and metal halides in the synthesis of lead sulfide quantum dots, the addition of sulfur sources is controlled to regulate the nucleation and growth of lead sulfide quantum dots, thus solving the waste of lead raw materials in the existing technology. and complex process problems, high-quality lead sulfide quantum dots were obtained, which are suitable for near-infrared solar cells and photodetectors.
Patent Information
- Application Number
- CN202210922624.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-08-02
AI Technical Summary
Among existing lead sulfide quantum dot synthesis methods, the high-temperature rapid injection method leads to waste of lead raw materials and product batch differences. The cation exchange method is complex and costly, and it is difficult to control the particle size and exciton absorption peak position.
Lead source, organic ligand, solvent and metal halide are mixed under vacuum heating to form a two-phase reaction system. A sulfur source is added to prepare lead sulfide quantum dots. The nucleation and growth process is controlled by the solid-liquid interface mass transfer rate to obtain uniform particle size. and high-quality quantum dots.
The preparation of lead sulfide quantum dots is achieved with safe operation, low cost and easy control. The particle size is uniform, the surface is well passivated, the exciton absorption peak peak to valley ratio is high, and the absorption half-width is narrow. It is suitable for near-infrared solar cells and photodetectors. .
Smart Images

Figure CN115287057B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor nanomaterials, and specifically relates to a method for preparing lead sulfide quantum dots, a near-infrared solar cell, and an application of a photoelectric detector. Background Art
[0002] Lead sulfide (PbS) quantum dots have the advantages of widely adjustable band gap, high quantum yield, high molar absorption coefficient and large exciton Bohr radius, and have great application prospects in the field of near-infrared solar cells and photodetectors. Device structure optimization and post-processing surface modification can effectively reduce intermediate defect states and improve solar cell performance. The latest certified energy conversion efficiency exceeds 13%. At the same time, PbS quantum dot near-infrared detection technology has also achieved rapid development, and key performance parameters such as specific detection rate, external quantum efficiency, response speed and dark current are comparable to indium gallium arsenide detectors. In addition, due to its advantages such as solution processability and no need for lattice matching, PbS quantum dots can be directly integrated with silicon-based wafers for the preparation of large-array imaging chips.
[0003] Material preparation, post-treatment surface modification and device structure design jointly determine the performance of PbS quantum dot devices. Most of the existing technical research focuses on the latter two, and there is little research on material preparation. At present, hexamethyldisilathione (TMS) is generally used as a sulfur source, which is quickly injected into a lead oleate solution at high temperature to synthesize PbS quantum dots. The existing technology has further developed the synthesis method of PbS quantum dots, using lead halide (PbX2) as a lead source to quickly inject oleylamine-sulfur at high temperature to generate PbS quantum dots. Both of these synthesis methods belong to hot injection methods. Sulfur precursors are quickly injected at high temperatures to immediately nucleate and generate PbS quantum dots. Only the lead source and sulfur source selected in the synthesis are different. In order to obtain high-quality PbS quantum dots, both methods select a high lead-sulfur ratio (Pb:S>8) for the initial feed, and the Pb:S ratios in the final generated PbS quantum dots are 1.3 and 1.8, respectively. Application in industrial production will cause a large amount of lead raw material waste, and at the same time produce high-concentration lead-containing waste liquid. The cation exchange synthesis process uses PbCl2 to continuously exchange ZnS (CdS) quantum dots, which undergo Oswald ripening to generate large-sized PbS quantum dots. The PbS quantum dot exciton absorption peak obtained by controlling the exchange time has a high peak-to-valley ratio and a narrow absorption half-width. However, the cation exchange method is a significant kinetic control process. The continuous injection of ZnS (CdS) quantum dots leads to the continuous growth of PbS quantum dots, which is not conducive to controlling the particle size of the product, and ultimately leads to product batch differences in the position of the exciton absorption peak of PbS quantum dots. In addition, the cation exchange method requires the preparation of ZnS (CdS) quantum dots before synthesizing PbS quantum dots, which increases the process flow and quantum dot purification process. At the same time, the PbS quantum dot preparation process is much longer than the hot injection method, and its application in industrial production will increase operating costs. Summary of the invention
[0004] The present invention provides a lead sulfide quantum dot preparation method, near-infrared solar cell, and photoelectric detector application. The method has the advantages of safe operation, simple controllability, low cost, and easy repeatability and amplification; the prepared quantum dots have uniform particle size, good surface passivation, high peak-to-valley ratio of exciton absorption peak, narrow absorption half-width, and high fluorescence quantum yield.
[0005] In a first aspect, the present invention provides a method for preparing lead sulfide quantum dots, comprising: mixing a lead source, an organic ligand, a solvent and a metal halide, and heating in a vacuum until the lead source is dissolved to obtain a two-phase reaction system, wherein the two-phase reaction system comprises a lead precursor solution and a solid phase insoluble substance; and adding a sulfur source to the two-phase reaction system to obtain lead sulfide quantum dots.
[0006] Among them, the step of mixing a lead source, an organic ligand, a solvent and a metal halide, and heating in vacuum until the lead source is dissolved to obtain a two-phase reaction system includes: mixing the lead source, an organic ligand, a solvent and a metal halide to obtain a first mixture; heating the first mixture in vacuum until the lead source is dissolved to obtain the two-phase reaction system; the step of adding a sulfur source to the two-phase reaction system to obtain lead sulfide quantum dots includes: introducing a protective gas, raising the temperature of the two-phase reaction system to a preset reaction temperature, and adding the sulfur source to obtain the lead sulfide quantum dots.
[0007] Among them, after the steps of introducing protective gas, raising the temperature of the two-phase reaction system to a preset reaction temperature, and adding the sulfur source, the method further comprises: keeping the temperature at the preset reaction temperature, adding a terminator, and rapidly cooling to room temperature to obtain a second mixture; and separating and purifying the second mixture to obtain the lead sulfide quantum dots.
[0008] Among them, the step of separating and purifying the second mixture to obtain the lead sulfide quantum dots includes: loading the second mixture into a preset number of centrifuge tubes, and adding precipitation liquid into the centrifuge tubes to precipitate the quantum dots to obtain a third mixture; centrifuging the third mixture and pouring off the supernatant; using nitrogen to blow off the residual solvent, and adding dispersion liquid to obtain the lead sulfide quantum dots.
[0009] Wherein, the lead source includes one or any combination of lead oxide, lead acetate, lead carbonate, lead oxalate and lead stearate; the organic ligand includes one or any combination of saturated or unsaturated fatty acids with a carbon atom number ≥ 8; the solvent includes octadecene; and the metal halide includes one or any combination of lead halide, cadmium halide, chromium halide and zinc halide.
[0010] Wherein, the protective gas includes one of nitrogen and argon.
[0011] Wherein, the preset reaction temperature is 80-180°C.
[0012] Wherein, the sulfur source includes hexamethyldisilathane.
[0013] Wherein, the terminator includes at least one of n-hexane, n-octane, chloroform and toluene.
[0014] The peak-to-valley ratio of the exciton absorption peak of the lead sulfide quantum dots is greater than 5, and the half-width of the absorption is less than 120 nm.
[0015] Among them, the molar volume ratio of the lead source to the organic ligand is 1:(1-4); the molar ratio of the metal halide to the lead source is greater than or equal to 0.3; and the molar ratio of the lead source to the sulfur source is (1-4):1.
[0016] In a second aspect, the present application provides a near-infrared solar cell photovoltaic device, comprising: a near-infrared solar cell photosensitive layer, the near-infrared solar cell photosensitive layer comprising lead sulfide quantum dots, and the lead sulfide quantum dots are prepared by any of the methods described above.
[0017] In a third aspect, the present application provides a photodetector, comprising: a photodetection photosensitive layer, wherein the photodetection photosensitive layer comprises lead sulfide quantum dots, and the lead sulfide quantum dots are prepared by any of the methods described above.
[0018] Different from the prior art, the preparation method of the present invention is to mix a lead source, an organic ligand, a solvent and a metal halide, and vacuum heat until the lead source is dissolved to obtain a two-phase reaction system, wherein the two-phase reaction system includes a lead precursor solution and a solid-phase insoluble substance; a sulfur source is added to the two-phase reaction system to obtain lead sulfide quantum dots. By adding a solid-phase medium to introduce a heterogeneous reaction system, the solid-liquid interface mass transfer rate inhibits the rapid diffusion of a highly active sulfur source, reduces the activity of the sulfur source, and matches the activity of the lead source and the sulfur source, thereby distinguishing between the two processes of nucleation and growth. The quantum dots finally prepared have uniform particle size, good surface passivation, high peak-to-valley ratio of exciton absorption peak, and narrow absorption half-height width. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of a process for preparing lead sulfide quantum dots according to an embodiment of the present invention;
[0020] Figure 2 This is a transmission electron microscope photo of the lead sulfide quantum dots prepared in Example 1;
[0021] Figure 3 Schematic diagram of absorption and fluorescence spectra of lead sulfide quantum dots prepared in Example 1;
[0022] Figure 4Schematic diagram of absorption spectra of lead sulfide quantum dots prepared in Example 1 at different holding times;
[0023] Figure 5 This is a transmission electron microscope photo of the lead sulfide quantum dots prepared in Example 2;
[0024] Figure 6 Schematic diagram of absorption and fluorescence spectra of lead sulfide quantum dots prepared in Example 2;
[0025] Figure 7 A schematic diagram of the structure of an embodiment of a near-infrared solar cell photovoltaic device;
[0026] Figure 8 FIG. 4 is a schematic structural diagram of an embodiment of a photoelectric detector. DETAILED DESCRIPTION
[0027] In order to explain the technical content, structural features, achieved purpose and effect of the technical solution in detail, the following is a detailed description in combination with specific embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0028] See also Figure 1 , is a schematic flow chart of an embodiment of a method for preparing lead sulfide quantum dots of the present invention, which specifically includes:
[0029] Step S11: Mix a lead source, an organic ligand, a solvent and a metal halide, and heat in a vacuum until the lead source is dissolved to obtain a two-phase reaction system.
[0030] The two-phase reaction system comprises a lead precursor solution and a solid phase insoluble substance.
[0031] Specifically, in one embodiment, a lead source, an organic ligand, a solvent and a metal halide are mixed to obtain a first mixture; the first mixture is vacuum heated until the lead source is dissolved to obtain the two-phase reaction system.
[0032] Step S12: adding a sulfur source into the two-phase reaction system to obtain lead sulfide quantum dots.
[0033] Specifically, a protective gas is introduced, the temperature of the two-phase reaction system is raised to a preset reaction temperature, and the sulfur source is added to obtain the lead sulfide quantum dots. In one embodiment, the reaction is kept warm at the preset reaction temperature for 0.01 to 2 hours; a terminator is added, and the mixture is quickly cooled to room temperature to obtain a second mixture; the second mixture is separated and purified to obtain the lead sulfide quantum dots.
[0034] In a specific embodiment, the second mixture is loaded into a preset number of centrifuge tubes, and a precipitating liquid is added to the centrifuge tubes to precipitate the quantum dots to obtain a third mixture; the third mixture is centrifuged and the supernatant is poured out; the residual solvent is blown dry with nitrogen, and a dispersion liquid is added to obtain the lead sulfide quantum dots.
[0035] The lead source includes one or any combination of lead oxide, lead acetate, lead carbonate, lead oxalate and lead stearate. The organic ligand includes one or any combination of saturated or unsaturated fatty acids with a carbon number of ≥8. For example, oleic acid. The solvent includes octadecene. The metal halide includes one or any combination of lead halide, cadmium halide, chromium halide and zinc halide.
[0036] In one embodiment, the protective gas includes one of nitrogen and argon. The precipitation liquid may be acetone.
[0037] It should be noted that the preset reaction temperature is 80-180°C.
[0038] In one embodiment, the sulfur source includes hexamethyldisilathane.
[0039] In one embodiment, the terminator includes at least one of n-hexane, n-octane, chloroform, and toluene.
[0040] It should be noted that the molar volume ratio of the lead source to the organic ligand is 1:(1-4); the molar ratio of the metal halide to the lead source is greater than or equal to 0.3; and the molar ratio of the lead source to the sulfur source is (1-4):1.
[0041] In one embodiment of the present application, a lead source, an organic ligand, a solvent and a metal halide are mixed in a reactor, the temperature is controlled at 100-120°C, and the vacuum is applied for 60-120 minutes until the lead source is completely dissolved to obtain a liquid lead precursor solution and a solid insoluble substance to form a two-phase reaction system; a protective gas is introduced into the reactor, the system temperature is maintained at 80-180°C, and a sulfur source is rapidly injected; the heat source is removed after keeping the reaction temperature for 0.01-2 hours, and then a terminator is added to quickly cool to room temperature, and the lead sulfide quantum dots are obtained after separation and purification.
[0042] In the present application, the peak-to-valley ratio of the exciton absorption peak of the lead sulfide quantum dots is greater than 5, and the half-width of the absorption is less than 120nm.
[0043] Embodiment 1:
[0044] (1) Preparation of TMS solution.
[0045] Add 210uL (1mmol) TMS to 1mL octadecene and mix well for later use. It should be noted that TMS solution is very volatile, so try to avoid leaving the prepared solution for a long time to reduce TMS loss.
[0046] (2) Preparation of lead sulfide quantum dots.
[0047] 405mg (1.8mmol) of lead source PbO, 139mg (0.5mmol) of metal halide PbCl2, 2mL of organic ligand oleic acid and 10mL of solvent octadecene are added to a three-necked flask with a condenser and stirred to obtain a first mixture. The first mixture is heated to 120°C under stirring and vacuumed for 1h. At this time, the yellow PbO is completely dissolved to form a clear and transparent lead oleate solution, while PbCl2 is still a solid powder, forming a two-phase reaction system, which includes a lead precursor solution and a solid insoluble substance. At this time, stop vacuuming, switch to a nitrogen atmosphere, heat to 150°C, and quickly inject the pre-configured sulfur source TMS solution after the temperature stabilizes. After keeping warm for 10min, remove the heat source, quickly inject 20mL of a terminator such as n-hexane into the flask to terminate the reaction, and quickly cool to room temperature.
[0048] (3) Purification.
[0049] Divide the solution in the flask into three 50mL centrifuge tubes, with about 10mL of solution in each centrifuge tube. Add 25-30mL of precipitation liquid such as acetone to each centrifuge tube to precipitate the quantum dots to obtain a turbid solution, and centrifuge at 9000rpm for 3min, pour off the supernatant, and use nitrogen to blow dry the residual solvent. Add 10mL of dispersion liquid such as n-hexane or toluene to the centrifuge tube to disperse the quantum dots, and repeat the above cleaning steps. Finally, store the obtained quantum dot powder in a glove box.
[0050] The lead sulfide quantum dots obtained in Example 1 were tested for microscopic morphology and optical properties. Figure 2 The transmission electron microscope photo of the prepared lead sulfide quantum dots is shown. Figure 2 It can be seen that the prepared quantum dot particle size distribution is uniform and the dispersion is good. According to the experimental data, the average particle size is about 5.2nm. Figure 3 Schematic diagram of absorption and fluorescence spectra of lead sulfide quantum dots prepared in Example 1, the first exciton absorption peak is at 1276nm, the absorption half-width is about 100nm, and the peak-to-valley ratio exceeds 5. The fluorescence peak wavelength is at 1370nm, and the half-width is about 150nm. Figure 4The absorption spectra of lead sulfide quantum dots prepared in Example 1 at different holding times are shown in Figure 1. It can be seen that the prepared lead sulfide quantum dots have good thermodynamic stability, and the peak-to-valley ratio and half-width of the absorption peak of the exciton absorption peak hardly change during the 60-min holding of the quantum dots after nucleation. The lead sulfide quantum dots obtained in Example 1 were dispersed in a tetrachloroethylene solution, and the QY value was measured to be about 40%.
[0051] Embodiment 2:
[0052] (1) Preparation of TMS solution.
[0053] Add 1 mL (5 mmol) of sulfur source TMS to 5 mL of octadecene and mix well for later use. It should be noted that TMS solution is very volatile, so try to avoid leaving the prepared solution for a long time to reduce TMS loss.
[0054] (2) Preparation of lead sulfide quantum dots.
[0055] 1115mg (5mmol) of lead source PbO, 695mg (2.5mmol) of metal halide PbCl2, 10mL of organic ligand oleic acid and 50mL of solvent octadecene were added to a three-necked flask with a condenser, nitrogen was introduced under stirring conditions, and the mixture was heated to 110°C and vacuumed for 2h. At this time, the yellow PbO was completely dissolved to form a clear and transparent lead oleate solution, while PbCl2 was still a solid powder, forming a heterogeneous reaction system. The mixture was stopped vacuuming, switched to a nitrogen atmosphere, heated to 150°C, and the pre-prepared TMS solution was quickly injected after the temperature stabilized. After keeping the temperature for 10min, the heat source was removed, and 40mL of toluene was quickly injected into the flask to terminate the reaction, and the mixture was quickly cooled to room temperature.
[0056] (3) Purification.
[0057] Divide the solution in the flask into 6 100mL centrifuge tubes, with about 20mL of solution in each centrifuge tube. Add about 50mL of acetone to each centrifuge tube to precipitate the quantum dots to obtain a turbid solution, and centrifuge at 9000rpm for 3min, pour off the supernatant, and use nitrogen to blow dry the residual solvent. Add 10mL of n-hexane or toluene to the centrifuge tube to disperse the quantum dots, and repeat the above cleaning steps. Finally, store the obtained quantum dot powder in a glove box.
[0058] The lead sulfide quantum dots obtained in Example 2 were tested for microscopic morphology and optical properties. Figure 5 The following is a transmission electron microscope photo of the prepared lead sulfide quantum dots. Figure 5 It can be seen that the prepared quantum dot particles have uniform size distribution and good dispersion, with an average particle size of about 7.4nm. Figure 6The absorption and fluorescence spectra of the prepared lead sulfide quantum dots are as follows: the first exciton absorption peak is at 1694 nm, the half-width of absorption is about 108 nm, and the peak-to-valley ratio is more than 6. The fluorescence peak wavelength is at 1728 nm, and the half-width is about 130 nm. The lead sulfide quantum dots obtained in Example 2 are dispersed in a tetrachloroethylene solution, and the QY value is measured to be about 10%.
[0059] Embodiment 3:
[0060] (1) Preparation of TMS solution.
[0061] 210uL (1mmol) TMS was added to 1mL octadecene and mixed evenly for later use. It should be noted that TMS solution is very volatile, so try to avoid leaving the prepared solution for a long time to reduce TMS loss.
[0062] (2) Preparation of lead sulfide quantum dots.
[0063] Add 405mg (1.8mmol) PbO, 278mg (1mmol) PbCl2, 2mL oleic acid and 10mL octadecene to a three-necked flask with a condenser, introduce nitrogen under stirring, heat to 120℃ and evacuate for 1.5h, at which time the yellow PbO is completely dissolved to form a clear and transparent lead oleate solution, while PbCl2 is still a solid powder, forming a heterogeneous reaction system. Stop evacuating, switch to nitrogen atmosphere, set the temperature to 100℃, and quickly inject the pre-prepared TMS solution after the temperature stabilizes. After keeping warm for 60min, remove the heat source, quickly inject 20mL n-hexane into the flask to terminate the reaction, and quickly cool to room temperature.
[0064] (3) Purification.
[0065] Divide the solution in the flask into three 50mL centrifuge tubes, with about 10mL of solution in each centrifuge tube. Add 25-30mL of acetone to each centrifuge tube to precipitate the quantum dots to obtain a turbid solution, and centrifuge at 9000rpm for 3min, pour off the supernatant, and use nitrogen to blow dry the residual solvent. Add 10mL of n-hexane or toluene to the centrifuge tube to disperse the quantum dots, and repeat the above cleaning steps. Finally, store the obtained quantum dot powder in a glove box.
[0066] Embodiment 4:
[0067] (1) Preparation of TMS solution.
[0068] 210uL (1mmol) TMS was added to 1mL octadecene and mixed evenly for later use. It should be noted that TMS solution is very volatile, so try to avoid leaving the prepared solution for a long time to reduce TMS loss.
[0069] (2) Preparation of lead sulfide quantum dots.
[0070] Add 682.8mg (1.8mmol) Pb (CH3COO) 2·3H2O, 91.7mg (0.5mmol) CdCl2, 2mL oleic acid and 10mL octadecene to a three-necked flask with a condenser, introduce nitrogen under stirring, heat to 120℃ and evacuate for 1h, at which time the yellow PbO is completely dissolved to form a clear and transparent lead oleate solution, while CdCl2 is still a solid powder, forming a heterogeneous reaction system. Stop evacuating, switch to nitrogen atmosphere, heat to 150℃, and quickly inject the pre-prepared TMS solution after the temperature stabilizes. After keeping warm for 20min, remove the heat source, quickly inject 20mL n-hexane into the flask to terminate the reaction, and quickly cool to room temperature.
[0071] (3) Purification.
[0072] Divide the solution in the flask into three 50mL centrifuge tubes, with about 10mL of solution in each centrifuge tube. Add 25-30mL of acetone to each centrifuge tube to precipitate the quantum dots to obtain a turbid solution, and centrifuge at 9000rpm for 3min, pour off the supernatant, and use nitrogen to blow dry the residual solvent. Add 10mL of n-hexane or toluene to the centrifuge tube to disperse the quantum dots, and repeat the above cleaning steps. Finally, store the obtained quantum dot powder in a glove box.
[0073] Embodiment 5:
[0074] (1) Preparation of TMS solution.
[0075] 210uL (1mmol) TMS was added to 1mL octadecene and mixed evenly for later use. It should be noted that TMS solution is very volatile, so try to avoid leaving the prepared solution for a long time to reduce TMS loss.
[0076] (2) Preparation of lead sulfide quantum dots.
[0077] Add 267.6mg (1.2mmol) PbO, 183.5mg (0.5mmol) PbBr2, 1mL oleic acid and 10mL octadecene to a three-necked flask with a condenser, introduce nitrogen under stirring, heat to 120℃ and evacuate for 1.5h, at which time the yellow PbO is completely dissolved to form a clear and transparent lead oleate solution, while PbBr2 is still a solid powder, forming a heterogeneous reaction system. Stop evacuating, switch to nitrogen atmosphere, heat to 150℃, and quickly inject the pre-prepared TMS solution after the temperature stabilizes. After keeping warm for 10min, remove the heat source, quickly inject 20mL of n-hexane into the flask to terminate the reaction, and quickly cool to room temperature.
[0078] (3) Purification.
[0079] Divide the solution in the flask into three 50mL centrifuge tubes, with about 10mL of solution in each centrifuge tube. Add 25-30mL of acetone to each centrifuge tube to precipitate the quantum dots to obtain a turbid solution, and centrifuge at 9000rpm for 3min, pour off the supernatant, and use nitrogen to blow dry the residual solvent. Add 10mL of n-hexane or toluene to the centrifuge tube to disperse the quantum dots, and repeat the above cleaning steps. Finally, store the obtained quantum dot powder in a glove box.
[0080] The present invention has the following advantages: the present invention has pioneered a heterogeneous synthesis method in the field of quantum dot material synthesis, which is significantly different from the traditional colloidal chemical synthesis method. By introducing a solid phase medium to balance the activity of anions and cations, high-quality lead sulfide quantum dots are prepared. The present invention is compatible with the advantages of existing preparation methods: safe operation, simple and controllable, low cost, easy to repeat and scale up; the prepared quantum dots have uniform particle size, good surface passivation, high exciton absorption peak-to-valley ratio, and high fluorescence quantum yield. The lead sulfide quantum dots prepared by the method of the present invention have great application prospects in the field of near-infrared solar cells and photodetectors.
[0081] See also Figure 7 and 8 , which is the formal ( Figure 7 ) and trans ( Figure 8 ) is a schematic diagram of a device structure, wherein the formal structure photosensitive layer 73 includes lead sulfide quantum dots, and the lead sulfide quantum dots are prepared by any method of the above-mentioned embodiments 1 to 5. The inverse structure photosensitive layer 84 includes lead sulfide quantum dots, and the lead sulfide quantum dots are prepared by any method of the above-mentioned embodiments 1 to 5.
[0082] Figure 7 The figure shows a schematic diagram of the structure of an embodiment of the near-infrared solar cell formal structure of the present invention. It should be noted that the functional layers of the near-infrared solar cell formal structure are, from top to bottom, respectively: a metal top electrode layer 71, a hole transport layer 72, a near-infrared solar cell photosensitive layer 73, an electron transport layer 74, and a bottom electrode layer 75. Among them, the hole transport layer 72 is a P-type hole transport layer, the electron transport layer 74 is an N-type electron transport layer, and the bottom electrode layer 75 is a transparent conductive material, such as ITO. After experiments, the photoelectric conversion efficiency of the infrared solar cell photovoltaic device under AM1.5 sunlight irradiation reached 12%.
[0083] Figure 8The figure shows a schematic diagram of the structure of an embodiment of the photodetector transverse structure of the present invention. It should be noted that the photodetector transverse structure includes, from bottom to top, a bottom electrode layer 87 (e.g., a transparent conductive bottom electrode ITO), a P-type hole transport layer 86, a P-type hole transition layer 85, a photodetection photosensitive layer 84, an N-type electron transition layer 83, an N-type electron transport layer 82, and a top electrode layer 81 (e.g., a transparent conductive top electrode ITO). According to the test, the external quantum efficiency of the detector reaches 60%, and the detection rate exceeds 10 12 Jones.
[0084] It should be noted that although the above embodiments have been described in this article, the patent protection scope of the present invention is not limited thereby. When the technical parameters and raw material components that are not described in detail are changed within the parameter range listed in the present invention, the same or similar technical effects as those of the above embodiments can still be obtained, and they still belong to the protection scope of the present invention. Therefore, based on the innovative concept of the present invention, the changes and modifications made to the embodiments described herein, or the equivalent structure or equivalent process transformation made by the contents of the specification and drawings of the present invention, directly or indirectly applying the above technical solutions to other related technical fields are all included in the patent protection scope of the present invention.
Claims
1. A method for preparing lead sulfide quantum dots, characterized in that: The preparation method comprises: A lead source, an organic ligand, a solvent and a metal halide are mixed, and vacuum heated until the lead source is dissolved to obtain a two-phase reaction system, wherein the two-phase reaction system includes a lead precursor solution and a solid phase insoluble substance; Adding a sulfur source into the two-phase reaction system to obtain lead sulfide quantum dots; The lead source includes one or any combination of lead oxide, lead acetate, lead carbonate, lead oxalate and lead stearate; The organic ligand includes one or any combination of saturated or unsaturated fatty acids having a carbon number ≥ 8; The solvent includes octadecene; The metal halide includes one or any combination of lead chloride, lead bromide and cadmium chloride.
2. The preparation method according to claim 1, characterized in that: The step of mixing a lead source, an organic ligand, a solvent and a metal halide, and heating in vacuum until the lead source is dissolved to obtain a two-phase reaction system comprises: Mixing a lead source, an organic ligand, a solvent and a metal halide to obtain a first mixture; Heating the first mixture under vacuum until the lead source is dissolved to obtain the two-phase reaction system; The step of adding a sulfur source to the two-phase reaction system to obtain lead sulfide quantum dots comprises: A protective gas is introduced, the temperature of the two-phase reaction system is raised to a preset reaction temperature, and the sulfur source is added to obtain the lead sulfide quantum dots.
3. The preparation method according to claim 2, characterized in that: After the steps of introducing the protective gas, raising the temperature of the two-phase reaction system to a preset reaction temperature, and adding the sulfur source, the method further comprises: Keeping the reaction temperature at the preset temperature, adding a terminator, and rapidly cooling the mixture to room temperature to obtain a second mixture; The second mixture is separated and purified to obtain the lead sulfide quantum dots.
4. The preparation method according to claim 3, characterized in that: The step of separating and purifying the second mixture to obtain the lead sulfide quantum dots comprises: The second mixture is placed into a preset number of centrifuge tubes, and a precipitating liquid is added into the centrifuge tubes to precipitate the quantum dots, thereby obtaining a third mixture; Centrifuging the third mixture and discarding the supernatant; The residual solvent is blown dry by nitrogen, and a dispersion liquid is added to obtain the lead sulfide quantum dots.
5. The preparation method according to claim 2, characterized in that: The protective gas includes one of nitrogen and argon.
6. The preparation method according to claim 2, characterized in that: The preset reaction temperature is 80-180°C.
7. The preparation method according to claim 2, characterized in that: The sulfur source includes hexamethyldisilathione.
8. The preparation method according to claim 3, characterized in that: The terminator includes at least one of n-hexane, n-octane, chloroform and toluene.
9. The preparation method according to claim 1, characterized in that: The lead sulfide quantum dots have an exciton absorption peak-to-valley ratio greater than 5, and an absorption half-width less than 120 nm.
10. The preparation method according to claim 2, characterized in that: The molar volume ratio of the lead source to the organic ligand is 1:(1-4); the molar ratio of the metal halide to the lead source is greater than or equal to 0.3; and the molar ratio of the lead source to the sulfur source is (1-4):1.
Citation Information
Patent Citations
Preparation method of lead sulfide quantum dot fluorescent powder
CN109850937A