A Cu-Bi-Mg / SiO2 catalyst and its preparation method and application
The preparation of Cu-Bi-Mg/SiO2 catalysts is solved through the co-precipitation method of Cu-Bi-Mg/SiO2 catalysts, and the problems of complex catalyst preparation and organic volatile emissions in the prior art are improved, thus improving the stability and filtration performance of the catalyst, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202211000659.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-19
AI Technical Summary
The preparation process of the existing 1,4-butyne glycol synthesis catalyst is complex and time-consuming, with organic volatile emission problems, and the catalyst is not easy to regenerate and recover, has a short life, and requires good filtration and separation performance in industrial applications.
Cu-Bi-Mg/SiO2 catalyst was prepared by co-precipitation method, and it was flashed and dried and calcined by silica sol to form a catalyst with a mesosphere morphology, avoiding the growth of CuO grains, increasing alkaline sites, and passing through microcrystals Magnesium oxide regulates pH, simplifies operating steps and reduces hetero ion introduction.
It achieves good stability and filtration performance of the catalyst, simplifies the preparation process, reduces harmful gas emissions, improves catalytic activity and flowability, and is suitable for industrial applications.
Smart Images

Figure BDA0003807242490000061 
Figure BDA0003807242490000071 
Figure HDA0003807242500000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supported catalysts, and specifically relates to a Cu-Bi-Mg / SiO 2 Catalyst, preparation method and application thereof. Background Art
[0002] 1,4-Butynediol is hydrogenated to obtain 1,4-butanediol (BDO). 1,4-Butanediol is an important basic organic chemical and fine chemical raw material, mainly consumed in polyurethane (PU), polybutylene terephthalate (PBT), γ-butyrolactone (GBL) and tetrahydrofuran (THF) and other fields. In recent years, my country's demand for 1,4-butanediol has continued to grow, and the production capacity by 2020 is about more than 2 million tons. As the country's requirements for the use of disposable biodegradable materials continue to increase, the demand for biodegradable materials PBAT and PBS continues to grow, which leads to the growing demand for its upstream raw material BDO. Domestic companies have newly expanded BDO units. BDO production capacity will be close to 8 million tons in a few years, and the demand for key catalysts for the production of 1,4-butynediol will also be further amplified.
[0003] In the 1940s, Reppe invented a process for synthesizing 1,4-butynediol using formaldehyde and acetylene as raw materials. This process uses copper acetylene as a catalyst, which increases the operating risk of acetylene and copper acetylene under reaction pressure. After the 1970s, a new catalyst for synthesizing 1,4-butynediol was developed, which improved the Reppe process. The catalyst used in this process is malachite, which has small particles and good activity. It reacts in a slurry bed, improves the operating pressure and reduces the risk of explosion. However, this catalyst is not resistant to wear, is easy to lose, and deactivates quickly. In response to this situation, acetylation catalysts with silica, zeolite, and diatomaceous earth as carriers later appeared. For example, patents US4288641 and US3920759 disclose supported catalysts for preparing 1,4-butynediol with formaldehyde and acetylene using molecular sieves and magnesium silicate as carriers, respectively. However, this type of catalyst has the following shortcomings: ⑴ It is not easy to regenerate and recycle, and has a short life; ⑵ The preparation process of molecular sieves and magnesium silicate carriers is relatively complicated and relatively expensive. Chinese patent CN112023963 uses micron-sized α-alumina as a carrier, and uses deposition precipitation method, co-impregnation method and other methods to load basic copper carbonate and basic bismuth carbonate onto the carrier multiple times (10 times). The preparation process is complicated, and the surface of α-alumina is relatively inert, and it is difficult for the active component of basic carbonate to interact with its surface, which will lead to uneven distribution of active components on the carrier, fewer active sites per unit surface area, and weak binding force, resulting in loss of active components. Chinese patents CN102950014, CN102950002 and CN103480382 all use SiO 2As the carrier, the active substance is basic copper bismuth carbonate, and then silica sol is added and spray-dried. The surface acidic SiO 2 Silicon with high content and no high temperature calcination is not stable enough in hydrothermal treatment for a long time, which may increase the loss of silicon in the product and may lead to the poisoning of the subsequent hydrogenation nickel catalyst. Chinese patent CN 106881097 first prepares silicon and aluminum precipitates, then adds copper and alkali in parallel, and adopts precipitation method or impregnation-deposition method to prepare. The catalyst preparation process includes precipitation or impregnation deposition, reduction, washing, vacuum freeze drying, calcination, etc. The process is relatively complicated and the equipment requirements are high. Chinese patent CN106669695 adopts a two-step precipitation process, that is, the solution of copper, bismuth and silicon and alkali are co-flowed to obtain a precipitate for the first time, and copper, bismuth and alkali are co-flowed to the precipitate obtained for the second time. After washing, silica sol is added for spray drying to obtain Cu-Bi / SiO 2 Catalyst. Chinese patent CN102658158 prepares copper, bismuth and magnesium salts into a solution, then adds organosilicon and organic solvent ethanol, hydrolyzes and precipitates under alkaline conditions, and then roasts in an inert atmosphere to obtain a Cu-Bi / C-MgO-SiO2 catalyst. This preparation method uses an organosilicon source, uses more ethanol, and roasts in an inert atmosphere. Chinese patent CN107952443 precipitates copper, bismuth, magnesium salt solution and silicon solution in water in parallel, washes and filters the precipitate, then pulps it, adjusts the pH to alkaline with alkali, washes, filters, pulps it, and performs a hydrothermal reaction for 30 to 50 hours, and finally filters, dries, roasts, and crushes it to obtain a catalyst with a certain particle size distribution.
[0004] The above methods for preparing supported 1,4-butynediol synthesis catalysts generally have the problems of complex and time-consuming preparation processes, or the emission of organic volatiles. In addition, the supported 1,4-butynediol synthesis catalysts need to have good filtration and separation performance in addition to good catalytic activity in industrial applications. Summary of the invention
[0005] The present invention aims to provide a Cu-Bi-Mg / SiO 2 A catalyst and a preparation method thereof and application in the synthesis of 1,4-butynediol.
[0006] Provide a Cu-Bi-Mg / SiO 2 The catalyst is composed of 25% to 45% silicon dioxide, 30% to 45% copper oxide, 5% to 18% magnesium oxide and the rest bismuth oxide in terms of mass percentage.
[0007] According to the above scheme, the catalyst is nearly spherical and has a particle size distribution of: 7 μm <D50<20μm。
[0008] According to the above scheme, the magnesium oxide in the catalyst is microcrystalline and highly dispersed in the crystalline CuO, which can effectively prevent the growth of CuO grains during calcination and increase the basic sites of the catalyst; preferably, the size of the CuO grains is 8 to 13 nm.
[0009] Provide a Cu-Bi-Mg / SiO 2 The method for preparing a catalyst comprises the following steps:
[0010] The coprecipitation method is adopted to precipitate a mixed solution of soluble copper salt, bismuth salt and magnesium salt, and silica sol is added to the obtained precipitate to carry out flash drying and then roasting to obtain the product.
[0011] According to the above scheme, the soluble copper salt is any one of copper sulfate, copper nitrate, and copper chloride, preferably copper nitrate; the soluble magnesium salt is any one of magnesium sulfate, magnesium nitrate, magnesium chloride, and magnesium acetate, preferably magnesium nitrate; the soluble bismuth salt is any one of bismuth sulfate, bismuth nitrate, bismuth chloride, and bismuth citrate, preferably bismuth nitrate.
[0012] According to the above scheme, the theoretically obtained Cu-Bi-Mg / SiO 2 The catalyst is the total amount, wherein, by mass percentage, the silica sol accounts for 25% to 45% of the total amount of the catalyst as silicon oxide, the water-soluble copper salt accounts for 30% to 45% of the total amount of the catalyst as copper oxide, the magnesium salt accounts for 5% to 18% of the total amount of the catalyst as magnesium oxide; and the bismuth salt is the remainder calculated as bismuth oxide.
[0013] According to the above scheme, the following steps are specifically included:
[0014] 1) Prepare water-soluble copper salt and magnesium salt to obtain Cu 2+ and Mg 2+ An acidic solution of bismuth salt is then added to obtain a Cu-Bi-Mg mixed acidic solution;
[0015] 2) mixing the alkaline solution and the Cu-Bi-Mg mixed acidic solution obtained in step 1) in a co-current manner under stirring conditions, controlling the pH of the system to be alkaline, and performing a precipitation reaction at 30-80° C. to obtain a precipitate;
[0016] 3) The precipitate obtained in step 2) is washed until it is nearly neutral and then filtered, and a certain amount of silica sol is added, stirred thoroughly, flash dried, and calcined to obtain a catalyst.
[0017] Preferably, in step 1), the nitric acid solution of the bismuth salt is prepared by dissolving the bismuth salt with a nitric acid solution and water, wherein the nitric acid solution is prepared by mixing concentrated nitric acid and water in a volume ratio of 1:1 to 1:4.
[0018] Preferably, in step 1), Cu2+ and Mg 2+ The acidic solution is prepared by dissolving a soluble copper salt in water, then adding a soluble magnesium salt to dissolve, and then adding acid to adjust the pH to 1-2 to obtain a solution containing Cu 2+ and Mg 2+ More preferably, the added acid is nitric acid or sulfuric acid.
[0019] Preferably, in step 2), the alkali in the alkali solution is one or a mixture of two of sodium carbonate, potassium carbonate, sodium hydroxide, potassium hydroxide, and sodium bicarbonate, more preferably sodium carbonate and sodium hydroxide.
[0020] Preferably, in step 2), the concentration of the alkali solution is 5% to 20% by mass.
[0021] Preferably, in step 2), the precipitation reaction temperature is 40°C to 75°C.
[0022] Preferably, in step 2), the precipitation method is to add the Cu-Bi-Mg mixed acid solution and the base into a stirred reaction vessel in parallel; the pH of the system is alkaline, which means that the pH of the system is 7.5 to 10.5, preferably 8.5 to 9.5.
[0023] Preferably, in step 3), the silica sol is acidic or alkaline, more preferably alkaline (pH < 10); the content of the silica sol is 10% to 30%, more preferably 20% to 30%.
[0024] Preferably, in step 3), the flash drying temperature is 160°C to 240°C, more preferably 190°C to 200°C; the solid content of the flash dried wet material is 30% to 60%, more preferably 35% to 45%;
[0025] Preferably, in step 3), the calcination temperature is 300°C to 550°C, and the calcination time is preferably 3 to 5 hours; more preferably, the calcination temperature is 350°C to 450°C.
[0026] Preferably, in step 3), washing is performed until the pH value is close to neutral, that is, pH ≤ 8.0.
[0027] Provide a Cu-Bi-Mg / SiO 2 The invention discloses an application of the catalyst in the synthesis of 1,4-butynediol, specifically, it is used for catalyzing the synthesis of 1,4-butynediol from formaldehyde and acetylene.
[0028] According to the above scheme, formaldehyde is an aqueous solution with a mass percentage concentration of 19% to 38%; the mass ratio of the catalyst to the formaldehyde solution is 1:15 to 1:12.
[0029] According to the above scheme, the catalyst is activated in advance, specifically: the catalyst is dispersed in a formaldehyde solution, and then acetylene gas is introduced under nitrogen protection for activation.
[0030] Preferably, the specific activation steps are: adding a catalyst and a 19% to 38% formaldehyde solution in a mass ratio of 1:15 to 1:12 to a jacketed reactor, introducing nitrogen and starting to heat up, and after sufficient replacement, when the temperature reaches 60°C to 70°C within 1 to 2 hours, cutting in acetylene gas so that acetylene accounts for 30% to 50% of the entire mixed gas, continuing to heat up, and cutting off nitrogen when the system temperature reaches 90°C, so that the acetylene gas is activated while ensuring excess, and the reaction continues for 6 to 12 hours. The activated catalyst is separated from the solution and reserved as a catalyst for synthesizing 1,4-butynediol.
[0031] The beneficial effects of the present invention are as follows:
[0032] 1. The present invention provides a Cu-Bi-Mg / SiO 2 The catalyst has crystalline copper oxide as the main active component, bismuth oxide as the auxiliary component, and microcrystalline magnesium oxide as a stabilizer for adjusting the acidity and base of the catalyst surface and dispersing the active components; when the catalyst is used to catalyze the reaction of formaldehyde and acetylene to prepare 1,4-butynediol, the catalyst first undergoes an oxidation-reduction reaction with formaldehyde to reduce divalent copper to monovalent copper, and further generates acetylide cuprous active substances. This process will produce acidic substances such as formic acid, which will enhance the acidity of the system; the microcrystalline and highly dispersed alkaline MgO in the catalyst has a certain effect of adjusting and stabilizing the pH of the system, so that the catalyst has good stability, and is also beneficial to the pH stability of the reaction system, which can reduce the regulation of pH, simplify the operation steps, and reduce the introduction of impurity ions. At the same time, the present invention has a nearly spherical particle morphology, good morphology stability, and the catalyst has good fluidity, dispersibility and filtration performance.
[0033] 2. The present invention provides a Cu-Bi-Mg / SiO 2The preparation method of the catalyst firstly uses a Cu-Bi-Mg mixed acid solution and an alkali co-current method to co-precipitate to prepare a Cu-Bi-Mg compound with a special structure. On the one hand, it can avoid the generation of bismuth silicate, copper silicate and other substances that are not conducive to the acetylation reaction when copper, bismuth, magnesium and silicon are co-precipitated together; on the other hand, it can make MgO exist between the active components in a highly dispersed microcrystalline form, which can inhibit the growth and aggregation of CuO grains during the calcination process of the catalyst, so that the active components have good dispersion and ensure high activity. In addition, the highly dispersed alkaline MgO with a microcrystalline structure has a certain function of regulating and stabilizing the pH of the system, so that the catalyst has good stability during the acetylation reaction. Further, silica sol is added to the Cu-Bi-Mg precipitation filter cake obtained by the co-precipitation method and mixed thoroughly, and the silica sol is used as a dispersing and molding binder, and is combined with rapid flash drying and molding, and the highly dispersed peptized SiO 2 Rapid water loss and bonding make the catalyst have a nearly spherical particle morphology with a relatively concentrated particle size distribution. The catalyst has good fluidity, dispersibility and filtration properties and is easy to use. The entire catalyst preparation process is relatively simple and has no harmful gas emissions, and has industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the morphology of the catalyst prepared in Example 3.
[0035] Figure 2 Comparison of the number of filtrations and the filtration time before the catalyst reaction in Example 3.
[0036] Figure 3 Comparison of the number of filtrations and the filtration time after the catalyst reaction in Example 3. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is further explained below through specific embodiments.
[0038] Example 1
[0039] Provide a Cu-Bi-Mg / SiO2 for synthesizing 1,4-butynediol 2 The method for preparing a catalyst comprises the following steps:
[0040] a. Weigh 60.2g of copper nitrate trihydrate and dissolve it in water. Then add 28.4g of magnesium nitrate hexahydrate and dissolve it. Add nitric acid to adjust the pH to 1.5.
[0041] b. Weigh 2.9 g of bismuth nitrate pentahydrate, add 3.0 ml of nitric acid solution (concentrated nitric acid and water volume ratio of 1:3) and 5 ml of water to dissolve, then add to the solution obtained in step a, add water to adjust the volume of the mixed solution to 250 ml to obtain a Cu-Bi-Mg mixed acidic solution.
[0042] c. Weigh 80 g of anhydrous sodium carbonate and add it to 320 g of water to obtain an alkali solution with a sodium carbonate mass percentage of 20%.
[0043] d. Add 100 ml of water to the flask, raise the temperature to 60°C, add the Cu-Bi-Mg mixed acidic solution obtained in step b and the alkaline solution obtained in step c in parallel under stirring, and control the pH of the suspension in the flask to 9.5±0.5. After 40±5 minutes of precipitation, age at a constant temperature for 40 minutes.
[0044] e. Wash the precipitate obtained in step d to a pH of ≤8.0, filter and obtain a filter cake.
[0045] f. Add water and 62 g of alkaline silica sol having a pH of 9 to 10 to the filter cake obtained in step e, wherein the silica content of the alkaline silica sol is 30%, and the solid content of the suspension is 35%, and stir well.
[0046] g. The wet material obtained in step f is flash dried at a drying air inlet temperature of 200°C to obtain a powder catalyst.
[0047] h. The powder obtained in step g was calcined at a temperature of 400°C for 3 hours to obtain a catalyst denoted as S1.
[0048] Example 2
[0049] Compared with Example 1, the only change is the solid content of the wet material after adding silica sol in step f, so that the solid content is 45%. The catalyst obtained in this way is recorded as S2.
[0050] Example 3
[0051] Compared with Example 1, the only change is that the precipitation temperature in step c is changed from 60° C. to 80° C., and the catalyst is recorded as S3.
[0052] in Figure 1 This is a morphology picture of the catalyst S3 prepared in Example 3. The picture shows that the catalyst has a nearly spherical morphology, 7 μm <D50<20μm;
[0053] Meanwhile, XRD test results show that the MgO in the obtained catalyst is microcrystalline and highly dispersed, and the CuO is crystalline, with a grain size of 8 to 13 nm.
[0054] Example 4
[0055] Compared with Example 1, the only change is that the alkali in step c is replaced by sodium hydroxide instead of sodium carbonate, and the mass percentage of the prepared alkali solution is 15%. The catalyst is recorded as S4.
[0056] Example 5
[0057] Compared with Example 4, the only change is that the precipitation temperature in step d is changed from 60°C to 75°C, and the catalyst is recorded as S5.
[0058] Example 6
[0059] Compared with Example 1, the only changes are that 60.2 g of copper nitrate trihydrate in step a is replaced by 62.2 g of copper sulfate pentahydrate; 28.4 g of magnesium nitrate hexahydrate is replaced by 23.3 g of magnesium sulfate pentahydrate, and the catalyst is recorded as S6.
[0060] The activity of the catalyst prepared in the above example was tested according to the above-mentioned 1,4-butynediol synthesis catalyst activity test method.
[0061] When carrying out the aldehyde-alkyne reaction, the catalyst of the present invention should be activated first, and the specific steps are:
[0062] Add a catalyst and 38% formaldehyde solution in a mass ratio of 1:12 to a jacketed reactor, introduce nitrogen and start heating. After sufficient replacement, when the temperature reaches 60°C to 70°C within 1 to 2 hours, cut in acetylene gas so that acetylene accounts for 30% to 50% of the entire mixed gas, continue to heat, and cut off nitrogen when the system temperature reaches 90°C, so that the acetylene gas is activated while ensuring excess, and the continuous reaction time is preferably 12 hours. The activated catalyst is separated from the solution and reserved as a catalyst for synthesizing 1,4-butynediol.
[0063] The activated catalyst was added to 38% formaldehyde for 12 hours, wherein the mass ratio of the catalyst (calculated before activation) to the 38% formaldehyde solution was 1:12. The results are shown in Table 1.
[0064] Table 1. Activity test results of prepared catalysts and industrial catalysts
[0065]
[0066] As can be seen from Table 1, the product yields of the catalysts prepared by the method of the present invention are better than those of industrial sample 1, and the product yields of Example 3, Example 4, and Example 5 are better than those of the industrial sample.
[0067] The following is the preparation method of Cu-Bi-Mg / SiO 2 The catalyst was tested for performance and the results are as follows:
[0068] During the activity test experiment of the catalyst prepared in Example 3 of the present invention, the pH value of the reactant system was basically stable, as shown in Table 2. This is due to the fact that the active component MgO with a special structure in the catalyst preparation in the example has appropriate alkalinity to timely regulate the acid generated when formaldehyde reduces copper during the synthesis of 1,4-butynediol.
[0069] Table 2 pH value of catalyst system at different reaction time
[0070]
[0071] The flash evaporation rapid drying molding preparation process technology used in the embodiment can obtain approximately spherical particles (see attached Figure 1 ), the catalyst has better dispersibility, fluidity and sedimentation in the formaldehyde solution reactant, which is beneficial to the gas-solid-liquid three-phase mass transfer in the 1,4-butynediol synthesis system.
[0072] In addition to having good catalytic activity, the 1,4-butynediol synthesis catalyst should also have good filtration separation performance in industrial applications. The fresh catalyst sample and the reaction sample were tested according to the following catalyst filtration performance test method. The filtration performance of the catalyst sample and the industrial catalyst sample in Example 3 of the present invention is shown in FIG. Figure 2 , Figure 3 shown.
[0073] Test method:
[0074] The filtration performance test of the catalyst uses an experimental G5 sand core funnel, and is equipped with 50 ml of a catalyst suspension with a certain particle size range distribution, in which the mass percentage of the catalyst is 10%. Under the suction filtration state, the stirred catalyst wet material is poured into the funnel for suction filtration at one time, and the time when the catalyst wet material is filtered out is recorded in time. After the first filtration, pour out the catalyst filter cake, rinse the catalyst on the sand core and slurry the filter cake together into the aforementioned suspension 50 ml, and continue the second filtration. Repeat the filtration operation for the subsequent 3 or 4 times to examine the filtration performance of the catalyst.
[0075] Figure 2 and Figure 3 As shown, from the 4 filtration data before and after the catalyst reaction, the filtration time of the catalyst sample of the present invention is shorter than that of the industrial sample, indicating that the catalyst prepared by the catalyst preparation method of the present invention has good filtration performance.
[0076] The embodiments of the specific preparation method of the catalyst of the present invention are not clauses to limit the preparation method of the present invention, and other similar expressions or replacements with the same meaning should fall within the scope of protection of this patent.
Claims
1. A Cu-Bi-Mg / SiO2 catalyst, characterized in that: The composition is as follows by mass percentage: 25% to 45% silicon dioxide, 30% to 45% copper oxide, 5% to 18% magnesium oxide, and the rest is bismuth oxide; wherein: The catalyst is nearly spherical; the magnesium oxide in the catalyst is microcrystalline and highly dispersed in the crystalline CuO; The catalyst is prepared by precipitating a mixed solution of soluble copper salt, bismuth salt and magnesium salt by a coprecipitation method, adding silica sol to the obtained precipitate, flash drying it and then calcining it.
2. The catalyst according to claim 1, characterized in that The particle size distribution of the catalyst is: 7µm <D50<20µm。 3. A method for preparing the Cu-Bi-Mg / SiO2 catalyst according to any one of claims 1 to 2, characterized in that: Bag The following steps are included: A coprecipitation method is used to precipitate a mixed solution of soluble copper salt, bismuth salt and magnesium salt, and the resulting precipitate is added The silica sol is flash dried and then calcined.
4. The preparation method according to claim 3, characterized in that: The soluble copper salt is any one of copper sulfate, copper nitrate, and copper chloride; the soluble magnesium salt is any one of magnesium sulfate, magnesium nitrate, magnesium chloride, and magnesium acetate; the soluble bismuth salt is any one of bismuth sulfate, bismuth nitrate, bismuth chloride, and bismuth citrate.
5. The preparation method according to claim 3, characterized in that: The theoretically obtained Cu-Bi-Mg / SiO2 catalyst is taken as the total amount, wherein, by mass percentage, the silica sol accounts for 25% to 45% of the total amount of the catalyst as silicon oxide, the water-soluble copper salt accounts for 30% to 45% of the total amount of the catalyst as copper oxide, the magnesium salt accounts for 5% to 18% of the total amount of the catalyst as magnesium oxide; and the bismuth salt is the remainder calculated as bismuth oxide.
6. The preparation method according to claim 3, characterized in that: The specific steps include: 1) Prepare water-soluble copper salt and magnesium salt to obtain Cu 2+ and Mg 2+ An acidic solution of bismuth salt is then added to obtain a Cu-Bi-Mg mixed acidic solution; 2) mixing the alkaline solution and the Cu-Bi-Mg mixed acidic solution obtained in step 1) in a co-current manner under stirring conditions, controlling the pH of the system to be alkaline, and performing a precipitation reaction at 30-80° C. to obtain a precipitate; 3) The precipitate obtained in step 2) is washed until it is nearly neutral and then filtered, and a certain amount of silica sol is added, stirred thoroughly, flash dried, and calcined to obtain a catalyst.
7. The preparation method according to claim 6, characterized in that: In the step 2), the pH of the system is controlled to be 7.5-10.5; and the precipitation reaction temperature is 40° C.-75° C.
8. The preparation method according to claim 6, characterized in that: In the step 3), the flash drying temperature is 160°C to 240°C, and the solid content of the flash dried wet material is 30% to 60%; the roasting temperature is 300°C to 550°C, and the roasting time is preferably 3 to 5 hours.
9. Use of the Cu-Bi-Mg / SiO2 catalyst according to any one of claims 1 to 2 in the synthesis of 1,4-butynediol, specifically: for catalyzing the synthesis of 1,4-butynediol from formaldehyde and acetylene.