A bismuth ferrite ceramic / glass composite material and its preparation method and application
By preparing bismuth ferrite ceramic/glass composite materials, combining the advantages of glass and ceramics, the problems of low dielectric constant and breakdown field strength of existing composite materials are solved, realizing the application of MLCCs with high dielectric performance and lead-free and environmentally friendly properties.
Patent Information
- Application Number
- CN202211111344.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-09-13
AI Technical Summary
Existing composite materials have low dielectric constants and breakdown field strengths, making them unsuitable for use in high-dielectric products.
Bismuth ferrite ceramic/glass composite material was prepared by sintering high-silicon lead-free glass with bismuth ferrite ceramic. Combining the advantages of B2O3-SiO2-BaO-Bi2O3 glass and (1-x)BiFeO3-xBaTiO3-ywt.%MnO2 ceramic, the resulting composite material was sintered at high temperature and normal pressure to form a composite material with good density.
The resulting composite material has high dielectric constant and Curie temperature, and high breakdown field strength, making it suitable for high-dielectric MLCC electronic products, and it does not contain the toxic element lead.
Smart Images

Figure CN115410832B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of composite materials for chip components, and more specifically, to a bismuth ferrite ceramic / glass composite material and a preparation method and application thereof. Background Art
[0002] Multilayer ceramic capacitors (MLCC) are one of the main chip components used in electronic equipment. They have large capacity, low equivalent resistance, excellent noise absorption, good pulse current resistance, small size, high insulation resistance, excellent impedance temperature characteristics and frequency characteristics, and good self-sealing properties. They can effectively prevent the internal electrodes from getting damp and contaminated, and significantly increase the arcing voltage and breakdown voltage. Therefore, they are widely used in information, military industry, mobile communications, electronics and electrical appliances, aviation, petroleum exploration and other industries.
[0003] In the development of electronic components, miniaturization is an eternal trend. Therefore, MLCC, which is used in large quantities and develops rapidly, is no exception. However, some MLCC products contain lead, which is highly volatile and destructive to the human body and the environment. For this reason, technicians in related fields are actively developing environmentally friendly products to replace MLCC. However, the environmentally friendly products developed are difficult to take into account the inherent small size and large capacity of MLCC. Related technology CN114315162A has developed a lead-free borosilicate glass-based ceramic composite material, which includes 40-60wt.% SiO as a matrix. 2 -B 2 O 3 -AlF 3 -SrO glass and 40-60wt.% of ceramics, a glass-based ceramic composite material is obtained by uniformly mixing ceramic powder with appropriate particle size with glass powder, granulating, pressing and sintering. It has been verified that when the glass-based ceramic composite material prepared by this method is applied to MLCC products, in addition to the advantages of small size and large capacity, it also has excellent microwave dielectric properties, low thermal expansion coefficient and high thermal conductivity. However, the dielectric constant and breakdown field strength of the composite material are low, and it can only be applied to low dielectric products, but not to high dielectric products.
[0004] Therefore, there is an urgent need to research a composite material that has a small size, large capacity, high dielectric constant and breakdown field strength, and can be used in high dielectric products. Summary of the invention
[0005] In order to solve the problem that the existing composite materials have low dielectric constant and breakdown field strength and cannot be applied to high dielectric products, the applicant has devoted himself to research and found that bismuth ferrite ceramics have a high dielectric constant, low dielectric loss and high Curie temperature, but the breakdown field strength is low. Glass has a high breakdown field strength and good sintering characteristics, which can perfectly make up for the defects of bismuth ferrite ceramics. To this end, the applicant has sintered high-silicon lead-free glass and bismuth ferrite ceramics through experiments to prepare a bismuth ferrite ceramic / glass composite material that can be used for MLCC high dielectric.
[0006] In a first aspect, the present application provides a bismuth ferrite ceramic / glass composite material, which adopts the following technical scheme: a bismuth ferrite ceramic / glass composite material, comprising 15-80wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass and 20-85wt.% (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics, where 0.3≤x≤0.4; 0.1≤y≤0.6.
[0007] By adopting the above technical solution, (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics have low dielectric loss and high dielectric constant and Curie temperature, but low breakdown field strength and high residual polarization strength; B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 (BSBB) glass has high breakdown field strength and low residual polarization intensity. After BSBB glass is melted into ceramics, it can perfectly compensate for (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 The defects of ceramics are eliminated, and the final composite material not only has a higher dielectric constant and Curie temperature, but also has a high breakdown field strength and low residual polarization strength, and can be used in high dielectric MLCC electronic products.
[0008] Preferably, the B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 The glass includes the following components in weight percentage: B 2 O3 :15-25wt.%、SiO 2 : 50-65wt.%, BaO: 5-10wt.% and Bi 2 O 3 :5-10wt.%.
[0009] Preferably, the (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Including the following raw materials: Bi 2 O 3 , Fe 2 O 3 、BaCO 3 、TiO 2 and MnO 2 .
[0010] In a second aspect, the present application provides a method for preparing a bismuth ferrite ceramic / glass composite material, using the following technical solution:
[0011] A method for preparing a bismuth ferrite ceramic / glass composite material comprises the following steps:
[0012] S1: B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 The raw materials of glass are ball-milled and mixed, and then dried, melted at high temperature, and quenched to obtain glass slag;
[0013] S2: The glass slag of S1 is ball milled to obtain BSBB glass powder; S3: (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 The ceramic ball is milled and mixed evenly, and then dried at high temperature to obtain ceramic raw material powder;
[0014] S4: the ceramic raw material powder obtained in S3 is subjected to high temperature sintering and ball milling to obtain ceramic powder;
[0015] S5: The glass powder obtained in S2 and the ceramic powder obtained in S4 are mixed, a binder is added, and the bismuth ferrite ceramic / glass composite material is obtained by granulation, tableting, debinding and sintering under high temperature and normal pressure atmosphere.
[0016] By adopting the above technical solution, BSBB glass powder has a higher breakdown field strength and a lower residual polarization strength. Through high-temperature melting and quenching, the obtained glass slag has a stable structure. (1-x)BiFeO 3-xBaTiO 3 -ywt.%MnO 2 Ceramics have a high dielectric constant and Curie temperature. After glass powder and ceramic powder are combined with a binder and sintered at high temperature and normal pressure, the resulting bismuth ferrite ceramic / glass composite material has good density and possesses the excellent properties of both ceramics and glass.
[0017] Preferably, in S1, the ball milling process uses ethanol as the solvent and zirconium balls as the ball milling medium, the diameter of the zirconium balls is 5-10 mm, and the mass ratio of the sum of the mass of the glass raw materials: ethanol: zirconium balls = 1:1:2-4; the high-temperature smelting temperature is 1500-1600°C, and the time is 0.5-2h.
[0018] Preferably, in S2, the glass slag obtained in S1 is ball-milled, and ethanol is used as a solvent and zirconium balls are used as ball-milling media in the ball-milling process. The diameters of the zirconium balls are different. In this step, the diameters of the zirconium balls are 12 mm, 8 mm and 2-4 mm. According to the mass ratio of the sum of the mass of the glass raw materials: ethanol: zirconium balls = 1:1:4, the particle size (D 50 ) is 0.1-10um on average.
[0019] Preferably, in S3, the ball milling process uses ethanol as the solvent and zirconium balls as the ball milling medium, the diameter of the zirconium balls is 5-10 mm, and the mass ratio of the sum of the mass of the glass raw materials: ethanol: zirconium balls is 1:1:2-4.
[0020] Preferably, in S4, the ceramic powder obtained in S3 is sintered at a high temperature of 800-850° C. and for a time of 1.5-2 h.
[0021] Preferably, in S4, the ceramic powder obtained in S3 is ball-milled, and ethanol is used as a solvent and zirconium balls are used as ball-milling media in the ball-milling process. The diameters of the zirconium balls are different. In this step, the diameters of the zirconium balls are 12 mm, 8 mm and 2-4 mm. According to the mass ratio of the sum of the mass of the glass raw materials: ethanol: zirconium balls = 1:1:2-4, the particle size (D 50 ) is 0.1-5.0um on average.
[0022] Preferably, the binder is polyvinyl butyral solution.
[0023] By adopting the above technical solution, polyvinyl butyral (PVB) has good adhesion to quartz glass. At the same time, it has the characteristics of transparency, heat resistance, cold resistance, high mechanical strength, etc., and is an excellent adhesive material for manufacturing laminated glass.
[0024] Preferably, in S5, the sintering temperature is 700-1000° C., the pressure is 10-4000 Pa, and the time is 10-120 min.
[0025] In a third aspect, the present application provides the use of bismuth ferrite ceramic / glass composite materials in the preparation of dielectric materials, using the following technical solutions:
[0026] Use of bismuth ferrite ceramic / glass composite materials in the preparation of high dielectric MLCCs.
[0027] In summary, this application has the following beneficial effects:
[0028] 1. The dielectric constant and Curie temperature of ceramics are high, but the breakdown field strength is low, while the breakdown field strength of glass is high. 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass and (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 The ceramic compound finally produces bismuth ferrite ceramic / glass composite material. After testing, it is found that this composite material combines the advantages of both ceramic and glass. It not only has high dielectric constant and Curie temperature, but also high breakdown field strength, and can be used in high dielectric MLCC electronic products.
[0029] Most of the materials on the market use BaTiO 3 Ceramics and PbTiO 3 Ceramics, BaTiO 3 The Curie temperature of ceramics is low and cannot be used in scenes with high temperature requirements. 3 Ceramics contain Pb elements, which will release toxicity during production and use. The B used in this application 2 O 3 -SiO 2 -BaO-Bi 2 O 3 (BSBB) glass material does not contain Pb element, but uses Si element instead of lead element, so the composite material obtained after compounding with ceramic is non-toxic, and the specific composition of ceramic is (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 When the two are combined, they form a bismuth ferrite ceramic / glass composite material with excellent performance.
[0030] 2. The existing ceramic sintering method is usually low-temperature and high-pressure sintering. However, in this application, after combining ceramics and glass, it was found that the density of the composite material obtained by low-temperature and high-pressure sintering was poor. Through continuous experiments, it was finally found that by using high temperature and normal pressure conditions, especially sintering a mixture of ceramics and glass at 700-1000℃ and 10-4000Pa parameters, a composite material with a high degree of densification can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a scanning electron microscope (SEM) image of the interior of the sample prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0032] The following is combined with Figure 1 The present application is further described in detail with reference to the accompanying drawings and embodiments.
[0033] Example
[0034] Example 1
[0035] In this embodiment, the bismuth ferrite ceramic / glass composite material includes 15wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 glass and 85wt.% (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 (x=0.33;y=0.55) ceramic. Among them, B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass consists of 15wt.% B 2 O 3 、65wt.%SiO 2 , 10wt.% BaO and 10wt.% Bi 2 O 3 Composition. (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 In ceramics, x is 0.33 and y is 0.55.
[0036] S1: Weigh B by mass 2 O 3 15g, SiO 2 65g, BaO 10g and Bi 2 O 310g, the weighed glass raw materials are mixed, and ethanol is used as a solvent for ball milling for 24h, the rotation speed is 300rpm, the ball milling medium is a zirconium ball with a diameter of 5mm, and the mass ratio is glass raw material: ethanol: zirconium ball = 1:1:4; the mixed raw materials are filtered and dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain glass raw material powder; the mixed glass raw material powder is high-temperature smelted at 1500℃ for 2h, and the glass melt is quenched in distilled water to obtain glass slag.
[0037] S2: The glass slag prepared in step 1 is crushed into glass powder by planetary ball milling at a speed of 800 rpm for 12 h; the ball milling medium is zirconium balls, the solvent is ethanol, and the mass ratio of glass slag: ethanol: zirconium balls is 1:1:4. In addition, zirconium balls are prepared in a mass ratio of 1:1:3 with diameters of 12 mm, 8 mm and 2 mm, respectively; the crushed glass powder is suspended in ethanol and filtered, and then dried at 100°C for 24 h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )1.0um BSBB glass powder.
[0038] S3: Weigh Bi by mass 2 O 3 33.7g, Fe 2 O 3 11.5g, BaCO 3 14.1g, TiO 2 5.7g and MnO 2 0.3575g, the weighed ceramic raw materials were mixed by planetary ball milling, the speed was 300rpm, the time was 12h; the ball milling medium was zirconium ball, the solvent was ethanol; the ceramic raw material: ethanol: zirconium ball = 1:1:4, the diameter of the zirconium ball was 5mm. The mixed raw materials were filtered, dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain ceramic raw material powder.
[0039] S4: The ceramic raw material powder prepared in S3 was sintered at 800°C for 2h and crushed by a planetary ball mill at a speed of 800rpm for 12h; the ball milling medium was zirconium balls and the solvent was ethanol; the ceramic raw material powder: ethanol: zirconium balls = 1:1:4, and the zirconium balls were mixed in a mass ratio of 1:1:3 with diameters of 12mm, 8mm and 2mm respectively; the crushed ceramic powder was suspended in ethanol and filtered, and then dried at 100°C for 24h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )0.5um (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic powder (x=0.33; y=0.55).
[0040] S5: Take the glass powder synthesized in S2 and the ceramic powder prepared in S4 and mix them in a high-speed mixer with ethanol as solvent for 20 minutes at a speed of 300 rpm. Take the mixed solution and filter it, dry it at 100℃ for 12 hours and pass it through a 200 mesh sieve to obtain a uniformly mixed ((1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.33; y=0.55) / glass mixture.
[0041] S6: Take the glass and ceramic powder mixture prepared in S5, add 1wt.% PVB solution of the same mass, then granulate, press and debind, and sinter for 10min at 700℃ and 10Pa to obtain (1-x)BiFeO with excellent performance. 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.33; y=0.55) / glass composite material.
[0042] Example 2
[0043] In this embodiment, the bismuth ferrite ceramic / glass composite material includes 30wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 glass and 70wt.% (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics. Among them, B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass consists of 25wt.% B 2 O 3 、65wt.%SiO 2 , 5wt.% BaO and 5wt.% Bi 2 O 3 Composition. (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 In ceramics, x is 0.3 and y is 0.6.
[0044] S1: Weigh B according to mass percentage 2 O 3 25g, SiO 2 65g, BaO 5g and Bi2 O 3 5g, the weighed glass raw materials are mixed, and ball milled with ethanol as a solvent for 24 hours at a rotation speed of 300rpm, the ball milling medium is zirconium balls with a diameter of 8mm, and the mass ratio is glass raw material: ethanol: zirconium balls = 1:1:3; the mixed raw materials are filtered and dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain glass raw material powder; the mixed glass raw material powder is high-temperature smelted at 1600℃ for 0.5h, and the glass melt is quenched in distilled water to obtain glass slag.
[0045] S2: The glass slag prepared in step 1 is crushed into glass powder by planetary ball milling at a speed of 800 rpm for 12 h; the ball milling medium is zirconium balls, the solvent is ethanol, and the mass ratio of glass slag: ethanol: zirconium balls is 1:1:4. In addition, zirconium balls are prepared in a mass ratio of 1:1:3 with diameters of 12 mm, 8 mm and 3 mm, respectively; the crushed glass powder is suspended in ethanol and filtered, and then dried at 100°C for 24 h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )0.1um BSBB glass powder.
[0046] S3: Weigh Bi according to mass ratio 2 O 3 35.2g, Fe 2 O 3 12.0g, BaCO 3 12.7 g, TiO 2 5.1g and MnO 2 0.39g, the weighed ceramic raw materials were mixed by planetary ball milling, the speed was 300rpm, the time was 12h; the ball milling medium was zirconium ball, the solvent was ethanol; the ceramic raw material: ethanol: zirconium ball = 1:1:2, the diameter of the zirconium ball was 10mm. The mixed raw materials were filtered, dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain ceramic raw material powder.
[0047] S4: The ceramic prepared in S3 was sintered at 800°C for 2h and crushed by a planetary ball mill at a speed of 800rpm for 12h; the ball milling medium was zirconium balls and the solvent was ethanol; the ceramic raw material powder: ethanol: zirconium balls = 1:1:3, and the zirconium balls were mixed in a mass ratio of 1:1:2 with diameters of 12mm, 8mm and 2mm respectively; the crushed ceramic powder was filtered by ethanol suspension, and then dried at 100°C for 24h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )5.0um (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic powder (x=0.3; y=0.6).
[0048] S5: Take the glass powder synthesized in S2 and the ceramic powder prepared in S4 and mix them in a high-speed mixer with ethanol as solvent for 20 minutes at a speed of 300 rpm. Take the mixed solution and filter it, dry it at 100℃ for 12 hours and pass it through a 200-mesh sieve to obtain a uniformly mixed (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.3; y=0.6) / glass mixture.
[0049] S6: Take the glass and ceramic powder mixture prepared in S5, add the same mass of 3wt.% PVB solution, then granulate, press and debind, and sinter at a temperature of 1000℃ and a pressure of 4000Pa for 50min to obtain (1-x)BiFeO with excellent performance. 3-x BaTiO 3-y wt.%MnO 2 (x=0.3; y=0.6) Ceramic / glass composite material.
[0050] Example 3
[0051] In this embodiment, the bismuth ferrite ceramic / glass composite material includes 50wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 glass and 50wt.% ((1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics. Among them, B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass consists of 25wt.% B 2 O 3 、55wt.%SiO 2 , 10wt.% BaO and 10wt.% Bi 2 O 3 Composition. (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 In ceramics, x is 0.4 and y is 0.3.
[0052] S1: Weigh B according to mass percentage 2 O 3 25g, SiO 255g, BaO 10g and Bi 2 O 3 10g, the weighed glass raw materials are mixed, and ethanol is used as a solvent for ball milling for 24h, the rotation speed is 300rpm, the ball milling medium is a zirconium ball with a diameter of 10mm, and the mass ratio is glass raw material: ethanol: zirconium ball = 1:1:2; the mixed raw materials are filtered and dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain glass raw material powder; the mixed glass raw material powder is high-temperature smelted at 1500℃ for 2h, and the glass melt is quenched in distilled water to obtain glass slag.
[0053] S2: The glass slag prepared in step 1 is crushed into glass powder by planetary ball milling at a speed of 800 rpm for 12 h; the ball milling medium is zirconium balls, the solvent is ethanol, and the mass ratio of glass slag: ethanol: zirconium balls is 1:1:4. In addition, zirconium balls are prepared in a mass ratio of 1:1:3 with diameters of 12 mm, 8 mm and 2 mm, respectively; the crushed glass powder is suspended in ethanol and filtered, and then dried at 100°C for 24 h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )10um BSBB glass powder.
[0054] S3: Weigh Bi according to mass ratio 2 O 3 30.4g, Fe 2 O 3 10.3g, BaCO 3 17g, TiO 2 6.9g and MnO 2 0.195g, the weighed ceramic raw materials were mixed by planetary ball milling, the speed was 300rpm, the time was 12h; the ball milling medium was zirconium ball, the solvent was ethanol; the ceramic raw material: ethanol: zirconium ball = 1:1:3, the diameter of the zirconium ball was 10mm. The mixed raw materials were filtered, dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain ceramic raw material powder.
[0055] S4: The ceramic raw material powder prepared in S3 was sintered at 800°C for 2h and crushed by a planetary ball mill at a speed of 800rpm for 12h; the ball milling medium was zirconium balls and the solvent was ethanol; the ceramic raw material powder: ethanol: zirconium balls = 1:1:2, and the zirconium balls were mixed in a mass ratio of 1:1:3 with diameters of 12mm, 8mm and 2mm respectively; the crushed ceramic powder was suspended in ethanol and filtered, and then dried at 100°C for 24h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )4.0um (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2Ceramic powder (x=0.4; y=0.3).
[0056] S5: Take the glass powder synthesized in S2 and the ceramic powder prepared in S4 and mix them in a high-speed mixer with ethanol as solvent for 20 minutes at a speed of 300 rpm. Take the mixed solution and filter it, dry it at 100℃ for 12 hours and pass it through a 200-mesh sieve to obtain a uniformly mixed (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.4; y=0.3) / glass mixture.
[0057] S6: Take the glass and ceramic powder mixture prepared in S5, add 5wt.% PVB solution of the same mass, then granulate, press and debind, and sinter at 900℃ and 1000Pa for 30min to obtain (1-x)BiFeO with excellent performance. 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.4; y=0.3) / glass composite material.
[0058] Example 4
[0059] In this embodiment, the bismuth ferrite ceramic / glass composite material includes 80 wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 glass and 20wt.% ((1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics. Among them, B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass consists of 20wt.% B 2 O 3 、60wt.%SiO 2 , 10wt.% BaO and 10wt.% Bi 2 O 3 Composition. (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 In ceramics, x is 0.4 and y is 0.1.
[0060] S1: Weigh B according to mass percentage 2 O 320g, SiO 2 60g, BaO 10g and Bi 2 O 3 10g, the weighed glass raw materials are mixed, and ethanol is used as a solvent for ball milling for 24h, the rotation speed is 300rpm, the ball milling medium is a zirconium ball with a diameter of 10mm, and the mass ratio is glass raw material: ethanol: zirconium ball = 1:1:2; the mixed raw materials are filtered and dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain glass raw material powder; the mixed glass raw material powder is high-temperature smelted at 1500℃ for 2h, and the glass melt is quenched in distilled water to obtain glass slag.
[0061] S2: The glass slag prepared in step 1 is crushed into glass powder by planetary ball milling at a speed of 800 rpm for 12 h; the ball milling medium is zirconium balls, the solvent is ethanol, and the mass ratio of glass slag: ethanol: zirconium balls is 1:1:4. In addition, zirconium balls are prepared in a mass ratio of 1:1:3 with diameters of 12 mm, 8 mm and 2 mm, respectively; the crushed glass powder is suspended in ethanol and filtered, and then dried at 100°C for 24 h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )5.0um BSBB glass powder.
[0062] S3: Weigh Bi according to mass ratio 2 O 3 30.4g, Fe 2 O 3 10.3g, BaCO 3 17g, TiO 2 6.9g and MnO 2 0.065g, the weighed ceramic raw materials were mixed by planetary ball milling, the speed was 300rpm, the time was 12h; the ball milling medium was zirconium ball, the solvent was ethanol; the ceramic raw material: ethanol: zirconium ball = 1:1:3, the diameter of the zirconium ball was 10mm. The mixed raw materials were filtered, dried at 100℃ for 24h, and then passed through a 100-mesh sieve to obtain ceramic raw material powder.
[0063] S4: The ceramic raw material powder prepared in S3 was sintered at 800°C for 2h and crushed by a planetary ball mill at a speed of 300rpm for 12h; the ball milling medium was zirconium balls and the solvent was ethanol; the ceramic raw material powder: ethanol: zirconium balls = 1:1:2, and the zirconium balls were mixed in a mass ratio of 1:1:3 with diameters of 12mm, 8mm and 2mm respectively; the crushed ceramic powder was suspended in ethanol and filtered, and then dried at 100°C for 24h and passed through a 200-mesh sieve to obtain an average particle size (D 50 )0.5um (1-x)BiFeO 3 -xBaTiO 3-ywt.%MnO 2 Ceramic powder (x=0.4; y=0.1).
[0064] S5: Take the glass powder synthesized in S2 and the ceramic powder prepared in S4 and mix them in a high-speed mixer with ethanol as solvent for 20 minutes at a speed of 300 rpm. Take the mixed solution and filter it, dry it at 100℃ for 12 hours and pass it through a 200-mesh sieve to obtain a uniformly mixed (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.4; y=0.1) / glass mixture.
[0065] S6: Take the glass and ceramic powder mixture prepared in S5, add 5wt.% PVB solution of the same mass, then granulate, press and debind, and sinter at 900℃ and 1000Pa for 30min to obtain (1-x)BiFeO with excellent performance. 3 -xBaTiO 3 -ywt.%MnO 2 Ceramic (x=0.4; y=0.1) / glass composite material.
[0066] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A bismuth ferrite ceramic / glass composite material, It is characterized in that Including 15-80wt.% B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 Glass and 20-85wt.% (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Ceramics; where 0.3≤x≤0.4; 0.1≤y≤0.6; The B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 The glass includes the following components in weight percentage: B 2 O 3 :15-25wt.%、SiO 2 : 50-65wt.%, BaO: 5-10wt.% and Bi 2 O 3 :5-10wt.%; The (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 Including the following raw materials: Bi 2 O 3 , Fe 2 O 3 、BaCO 3 、TiO 2 and MnO 2 The method for preparing the bismuth ferrite ceramic / glass composite material comprises the following steps: S1: B 2 O 3 -SiO 2 -BaO-Bi 2 O 3 The raw materials of glass are mixed and ball-milled, dried, melted at high temperature, and quenched to obtain glass slag; S2: BSBB glass powder is prepared by ball milling the glass slag of S1; S3: (1-x)BiFeO 3 -xBaTiO 3 -ywt.%MnO 2 The ceramic ball is milled and mixed evenly, and then dried at high temperature to obtain ceramic raw material powder; S4: the ceramic raw material powder obtained in S3 is subjected to high temperature sintering and ball milling to obtain ceramic powder; S5: mixing the glass powder obtained in S2 and the ceramic powder obtained in S4, adding a binder, and granulating, tableting, debinding, and sintering under high temperature and normal pressure to obtain the bismuth ferrite ceramic / glass composite material; The temperature of the S1 high temperature smelting is 1500-1600°C and the time is 0.5-2h; The sintering temperature in S5 is 700-1000° C. and the pressure is 10-4000 Pa.
2. The bismuth ferrite ceramic / glass composite material according to claim 1, It is characterized in that The average particle size of the BSBB glass powder prepared in S2 is 0.1-10 um.
3. The bismuth ferrite ceramic / glass composite material according to claim 1, It is characterized in that The average particle size of the ceramic powder prepared in S4 is 0.1-5 um.
4. The bismuth ferrite ceramic / glass composite material according to claim 1, It is characterized in that The binder is polyvinyl butyral solution.
5. Use of the bismuth ferrite ceramic / glass composite material according to any one of claims 1 to 4 in the preparation of dielectric materials, It is characterized in that Use in the preparation of high dielectric MLCC.