A method for washing anode mud containing precious metal nickel
Through the methods of mechanical screening, slurry washing and press filter dehydration, the problems of nickel loss, difficulty in handling residual electrode blocks and high labor intensity in the treatment of nickel anode sludge are solved, and efficient recovery and clean production of nickel anode sludge are achieved. Improved working environment.
Patent Information
- Application Number
- CN202211042769.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-08-29
AI Technical Summary
The existing nickel anode mud treatment process has problems such as nickel loss, difficulty in handling residual electrode blocks, high labor intensity, high moisture content, and blockage of the delivery pump pipeline.
It adopts the methods of mechanical screening, slurry washing, multi-stage booster pump transportation and filter press dehydration, through grid screening, inclined screen screening, double-layer stirring, filter press filtering and multiple nickel enrichment cycles. , respectively recover nickel ions and residual electrode blocks in the nickel anode mud, and reduce the water content and hydrophobicity of the nickel anode mud.
Effectively recover nickel ions and residual electrode blocks, reduce the nickel and moisture content of nickel anode mud, reduce manual labor intensity, improve the working environment, and achieve clean and civilized production of anode mud.
Smart Images

Figure CN115465903B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nickel electrolysis, and more specifically to the technical field of a method for washing anode mud containing precious metal nickel. Background Art
[0002] Nickel anode mud refers to a substance with metallic properties composed of sulfur and precious metals as the main elements produced in the electrolysis of soluble anode nickel. During the electrolysis of soluble anodes, the insoluble components of the anode settle to the bottom of the electrolytic cell as nickel anode mud, and the nickel anode mud is recovered from the electrolytic cell when the anode is replaced. During electrolysis, base metals with a more negative potential enter the solution, and precious metals, scattered metals (such as selenium, bismuth, etc.), anode powder, etc. form insoluble substances to become nickel anode mud. The main components of nickel anode mud are Ni: 2.17%, Cu: 0.22%, Co: 0.06%, S: 92.10%, H20: 29.14%, Au: 42.13g / t, Pd: 55.42g / t, Pt: 45.45g / t, Ag: 1.44g / t, trace amounts of platinum group metals, platinum group metals, gold and a small amount of silver in metallic state.
[0003] The main process for treating nickel anode mud is pyrometallurgy. Pyrometallurgy is to roast nickel anode mud at high temperature to produce liquid sulfur. At present, the treatment method of nickel anode mud is to manually scrape the anode mud into the hopper, let it stand for 24 hours, control part of the anode liquid (nickel sulfate solution) contained in the nickel anode mud, and transport it to the material yard of the precious metal enrichment workshop by agricultural vehicles.
[0004] The problems existing in the existing nickel anode mud operation process are:
[0005] (1) The nickel solution in the nickel anode mud is not further recovered by washing, and the nickel anode mud still contains a relatively high amount of anolyte, resulting in nickel loss;
[0006] (2) There are residual anode blocks in the nickel anode mud. During the manual loading process, not all the residual anode blocks can be picked out. Some residual anode blocks are mixed in the nickel anode mud, which increases the difficulty of downstream processing;
[0007] (3) The manual loading of nickel anode mud after water control is labor-intensive;
[0008] (4) Solution spillage during vehicle transportation;
[0009] (5) Nickel anode mud is highly hydrophobic, and liquid-solid separation is likely to occur during the slurry washing process. At the same time, the transportation of nickel anode mud is likely to cause blockage of the delivery pump and pipeline. Summary of the invention
[0010] The purpose of the present invention is to solve the technical problems of waste of metallic nickel, increased difficulty in handling downstream processes due to residual anode blocks, high labor intensity and high water content of nickel anode mud in the above-mentioned existing nickel anode mud operation process, and provide a method for washing anode mud containing precious metal nickel.
[0011] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0012] A method for washing anode mud containing precious metal nickel comprises the following steps:
[0013] Step 1: Screening of nickel anode mud: first, use a screening machine with a grid aperture of 20-40 mm to perform a primary screening to obtain a primary screening material, and then put the primary screening material into an inclined screen with a screening aperture of 2-4 mm for secondary screening to obtain a screening material;
[0014] Step 2: washing the nickel anode mud, adding the screened material obtained in step 1 into a slurry tank, adding clean water into the slurry tank, the mass ratio of the screened material to the clean water is 1:2.5-4, the screened material and the clean water in the slurry tank are fully stirred and slurried at 100-130 r / min to obtain a slurry washing mixed solution;
[0015] Step 3: transporting the nickel anode mud, using a multi-stage booster pump to transport the slurry washing mixed liquid obtained in step 2 from the slurry tank to the filter press, and the outlet pressure of the multi-stage booster pump is 0.3 MPa;
[0016] Step 4: dehydration of the nickel anode mud, the slurry washing mixed liquid transported to the filter press in step 3 is placed in the filter press, the pressure is controlled at 1-1.2 MPa, and the filter is filtered for 0.25-0.75 h, the washing liquid and the filter residue are collected respectively, and the filter residue is blown for 15 min to obtain sulfur-rich anode mud;
[0017] Step 5: enrichment of nickel anode mud washing liquid. Add the washing liquid obtained in step 4 into the slurry tank, repeat the operations of step 2 to step 4, and the washing liquid undergoes multiple nickel enrichment cycles to obtain a washing liquid rich in nickel ions.
[0018] Preferably, the stirring method in step 2 is double-layer stirring.
[0019] Preferably, the double-layer stirring includes three-slanted blade axial flow stirring in the upper layer and three-slanted blade radial flow stirring in the lower layer.
[0020] Preferably, the volume ratio of the sieved product to clean water or washing liquid in step 2 is 1:3.
[0021] Preferably, the nickel anode slurry washing time in step 2 is 0.3-0.8h, and the temperature is 50-60°C.
[0022] Preferably, the nickel anode slurry washing time in step 2 is 0.5h.
[0023] Preferably, the bottom of the slurry tank in step 3 is configured to be sloped.
[0024] Preferably, the slope of the bottom of the slurry tank is 3°.
[0025] Preferably, the screen in step 1 is tiltedly arranged in the slurry tank, and a slag removal opening is arranged at the lower end of the screen.
[0026] The beneficial effects of the present invention are as follows:
[0027] 1. The present invention solves the problems of waste of metallic nickel, increased difficulty in handling downstream processes due to residual anode blocks, high manual labor intensity and high water content of nickel anode mud in the existing nickel anode mud operation process by mechanically screening, washing, conveying, dehydrating and performing nickel enrichment process operations on nickel anode mud. The anode mud obtained by filtration by a filter press can be directly fed into a sulfur melting kettle for roasting to produce liquid sulfur, so that the purpose of preventing the anode mud from falling to the ground is achieved, and clean and civilized production is realized on site. The washing method of the present invention reduces the nickel and water content of the nickel anode mud, effectively recovers nickel sulfate solution and residual anode blocks, and at the same time reduces manual labor intensity and improves the working environment.
[0028] 2. Nickel anode mud contains a small amount of electrolytic residual blocks and insoluble particles. It is necessary to use secondary screening to recover the residual blocks and larger particles respectively to ensure that there are no larger particles in the nickel anode mud and reduce the impact on the roasting of the downstream nickel anode mud in the molten sulfur kettle; the first screening is mechanical screening, which mainly removes the electrolytic residual blocks, and the second screening is carried out in the nickel anode mud slurry tank, which mainly removes small pieces of residue and polymerized sulfur particles in the nickel anode mud; at the same time, nickel anode mud is extremely hydrophobic. In order to avoid the rapid sedimentation of nickel anode mud and improve the washing efficiency, slurry washing adopts double-layer stirring, which mainly solves the problem of easy sedimentation and transportation of nickel anode mud and achieves the purpose of efficient washing. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The figure is a schematic flow chart of the method for washing anode mud containing precious metal nickel according to the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0031] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for washing anode mud containing precious metal nickel, comprising the following steps:
[0034] Step 1: Screening of nickel anode mud: first, use a screening machine with a grid aperture of 30 mm to screen sample 1 once to obtain a primary screening material, and then put the primary screening material into an inclined screen with a screening aperture of 3 mm for secondary screening to obtain a screening material;
[0035] Step 2: Washing of nickel anode mud: add 2000 kg of the screened material obtained in step 1 into a slurry tank of Φ2500×3000 mm, add 6000 kg of clean water into the slurry tank, the mass ratio of the screened material to the clean water is 1:3, fully stir and slurry wash the screened material and the clean water in the slurry tank at 120 r / min, the slurry washing time is 0.5 h, and the temperature is 55°C. Obtain a slurry washing mixed solution;
[0036] Step 3: transporting the nickel anode mud, using a multi-stage booster pump to transport the slurry washing mixed liquid obtained in step 2 from the slurry tank to the filter press, and the outlet pressure of the multi-stage booster pump is 0.3 MPa;
[0037] Step 4: dehydration of nickel anode mud, the slurry washing mixed liquid transported to the filter press in step 3 is placed in the filter press, the pressure is controlled at 1.1 MPa, and the filter is filtered for 0.5 h, the washing liquid and the filter residue are collected respectively, the filter residue is blown for 15 min to obtain sulfur-rich anode mud, and the sulfur content (%) and water content (%) in the anode mud are determined;
[0038] Step 5: enrichment of nickel anode mud washing liquid. Add the washing liquid obtained in step 4 into the slurry tank, repeat the operations from step 2 to step 4, and the washing liquid is cycled through nickel enrichment for 9 times. After each cycle of washing, collect the washing liquid to determine the Ni ion concentration (g / L).
[0039] The measurement results of step 4 and step 5 are shown in Table 1.
[0040] Table 1 Nickel anode mud washing liquid circulation washing test washing liquid and slag composition (g / L, %) of sample 1
[0041]
[0042]
[0043] As shown in Table 1, during the washing process of sample 1, as the nickel content of the nickel anode mud washing liquid gradually increased, the nickel content of the washing residue gradually increased. In the sixth batch of the test, the nickel content of the washing liquid was enriched to 38.38g / L, and the nickel content of the washing residue increased to 0.89%; in the tenth batch of the test, the nickel content of the washing liquid was enriched to 52.29g / L, and the nickel content of the washing residue increased to 1.28%. After the eighth batch, the nickel ion in the washing liquid was enriched to 44.67g / L, and the nickel content of the washing residue was ≤1.18%, and the water content was ≤10.01%.
[0044] Example 2
[0045] This embodiment provides a method for washing anode mud containing precious metal nickel, comprising the following steps:
[0046] Step 1: Screening of nickel anode mud: first, use a screening machine with a grid aperture of 20 mm to screen sample 2 once to obtain a primary screening material, and then put the primary screening material into a sieve with a screening aperture of 2 mm for secondary screening to obtain a screening material;
[0047] Step 2: washing the nickel anode mud, adding the screened material obtained in step 1 into a slurry tank, adding clean water into the slurry tank, the mass ratio of the screened material to the clean water being 1:2.5, and fully stirring and slurry washing the screened material and the clean water in the slurry tank at 100 r / min to obtain a slurry washing mixed solution;
[0048] Step 3: transporting the nickel anode mud, using a multi-stage booster pump to transport the slurry washing mixed liquid obtained in step 2 from the slurry tank to the filter press, and the outlet pressure of the multi-stage booster pump is 0.3 MPa;
[0049] Step 4: dehydration of nickel anode mud, the slurry washing mixed liquid transported to the filter press in step 3 is placed in the filter press, the pressure is controlled at 1MPa, and the filter is filtered for 0.75h, the washing liquid and the filter residue are collected respectively, the filter residue is blown for 20min to obtain sulfur-rich anode mud, and the sulfur content (%) and water content (%) in the anode mud are determined;
[0050] Step 5: enrichment of nickel anode mud washing liquid. Add the washing liquid obtained in step 4 into the slurry tank, repeat the operations from step 2 to step 4, and the washing liquid is cycled through nickel enrichment for 9 times. After each cycle of washing, collect the washing liquid to determine the Ni ion concentration (g / L).
[0051] The measurement results of step 4 and step 5 are shown in Table 2.
[0052] Table 2 Nickel anode mud washing liquid circulation washing test washing liquid and slag composition (g / L, %) of sample 2
[0053]
[0054] As shown in Table 2, during the washing process of sample 2, as the nickel content of the nickel anode mud washing liquid gradually increased, the nickel content of the washing residue gradually increased. In the sixth batch of the test, the nickel content of the washing liquid was enriched to 38.87g / L, and the nickel content of the washing residue increased to 0.91%; in the tenth batch of the test, the nickel content of the washing liquid was enriched to 53.39g / L, and the nickel content of the washing residue increased to 1.35%. After the eighth batch, the nickel ion in the washing liquid was enriched to 45.12g / L, and the nickel content of the washing residue was ≤1.17%, and the water content was ≤9.55%.
[0055] Example 3
[0056] This embodiment provides a method for washing anode mud containing precious metal nickel, comprising the following steps:
[0057] Step 1: Screening of nickel anode mud: first, use a screening machine with a grid aperture of 40 mm to screen sample 3 once to obtain a primary screening material, and then put the primary screening material into a sieve with a screening aperture of 4 mm for secondary screening to obtain a screening material;
[0058] Step 2: washing the nickel anode mud, adding the screened material obtained in step 1 into a slurry tank, adding clean water into the slurry tank, the mass ratio of the screened material to the clean water being 1:4, fully stirring and slurry washing the screened material and the clean water in the slurry tank at 130 r / min, to obtain a slurry washing mixed solution;
[0059] Step 3: transporting the nickel anode mud, using a multi-stage booster pump to transport the slurry washing mixed liquid obtained in step 2 from the slurry tank to the filter press, and the outlet pressure of the multi-stage booster pump is 0.3 MPa;
[0060] Step 4: dehydration of nickel anode mud, the slurry washing mixed liquid transported to the filter press in step 3 is placed in the filter press, the pressure is controlled at 1.2 MPa, and the filter is filtered for 0.25 h, the washing liquid and the filter residue are collected respectively, the filter residue is blown for 18 min to obtain sulfur-rich anode mud, and the sulfur content (%) and water content (%) in the anode mud are determined;
[0061] Step 5: enrichment of nickel anode mud washing liquid. Add the washing liquid obtained in step 4 into the slurry tank, repeat the operations of step 2 to step 4, and the washing liquid is subjected to multiple nickel enrichment cycles. After each washing cycle, collect the washing liquid to determine the Ni ion concentration (g / L).
[0062] The measurement results of step 4 and step 5 are shown in Table 3.
[0063] Table 3 Nickel anode mud washing liquid circulation washing test washing liquid and slag composition (g / L, %) of sample 3
[0064]
[0065] As shown in Table 3, during the washing process of sample 3, as the nickel content of the nickel anode mud washing liquid gradually increased, the nickel content of the washing residue gradually increased. In the sixth batch of the test, the nickel content of the washing liquid was enriched to 37.86g / L, and the nickel content of the washing residue increased to 0.95%; in the eighth batch of the test, the nickel content of the washing liquid was enriched to 44.22g / L, and the nickel content of the washing residue increased to 1.25%. After the eighth batch, the nickel ion in the washing liquid was enriched to 44.22g / L, and the nickel content of the washing residue was ≤1.25%, and the water content was ≤10%.
[0066] In summary, the washing method of the present invention reduces the nickel and water content of nickel anode mud. After the eighth batch, the nickel ion in the washing liquid is enriched to more than 45g / L, the nickel content of the washing slag is ≤1.1%, and the water content is ≤10%. The nickel sulfate solution and the residual anode blocks are effectively recovered, and the entire cleaning process is mechanically operated to achieve the goal of preventing the anode mud from falling to the ground, reducing the labor intensity of the workers, achieving clean and civilized production on site, and improving the working environment.
Claims
1. A method for washing anode mud containing precious metal nickel, characterized in that: It includes the following steps: Step 1: Screening of nickel anode mud: First, use a screening machine with a grid aperture of 20-40 mm to screen the primary sieve. The obtained primary sieve undersize is placed on a sieve with a sieve aperture of 2-4 mm for secondary sieving to obtain the sieve undersize; Step 2: Washing of nickel anode mud: Add the undersize obtained in step 1 to the slurry tank, add clean water to the slurry tank, and wash the undersize. The mass ratio of the undersize to the clean water is 1:2.5~4. The undersize and the clean water in the slurry tank are fully stirred at 100~130r / min. Slurry washing to obtain a slurry washing mixed liquid; Step 3: Transportation of nickel anode mud: using a multi-stage booster pump to mix the slurry obtained in step 2 in the slurry tank. The liquid is transported to the filter press, and the outlet pressure of the multi-stage booster pump is 0.3MPa; Step 4: Dehydration of nickel anode mud: the slurry washing mixed liquid transported to the filter press in step 3 is placed in the filter press. Control the pressure at 1~1.2MPa, filter for 0.25~0.75h, collect the washing liquid and filter residue respectively, and blow the filter residue for 15~20min. Processing to obtain sulfur-rich anode mud; Step 5: Enrichment of nickel anode mud washing liquid: Add the washing liquid obtained in step 4 into the slurry tank, and repeat steps 2 to In the operation of step 4, the washing liquid is subjected to multiple nickel enrichment cycles to obtain a washing liquid rich in nickel ions; The mass ratio of the sieve material to the clean water or washing liquid in step 2 is 1:3; The nickel anode slurry washing time in step 2 is 0.3-0.8h, and the temperature is 50-60°C; The nickel anode slurry washing time in step 2 is 0.5h; The stirring method in step 2 is double-layer stirring; The double-layer stirring includes three-slanted blade axial flow stirring in the upper layer and three-slanted blade radial flow stirring in the lower layer; In step 3, the bottom of the slurry tank is set to be sloped; The slope of the bottom of the slurry tank is 3°; In step 1, the screen is tiltedly arranged in the slurry tank, and a slag removal opening is arranged at the lower end of the screen.
Citation Information
Patent Citations
Method for desulfurizing few samples of nickel anode slime