A method for efficiently preparing ferrous oxalate using red mud

Through the combination of low-concentration hydrochloric acid-oxalic acid two-stage grading acid leaching process and ascorbic acid reducing agent, the spiral winding microchannel reaction system was used to solve the problem of large acid consumption and impurity ions recovery in red mud, and ferrous oxalate was realized. Efficient preparation and environmentally friendly resource utilization.

CN115466174BActive Publication Date: 2024-12-03CHONGQING UNIV OF ARTS & SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211034693.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-12-03
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

The existing iron recovery technology in red mud has problems such as high inorganic acid consumption, unfriendly environment, and impurity ions coexistence and leaching. In addition, iron in the iron-containing oxalic acid solution leaching oxalic acid is in the form of Fe2+ and Fe3+ ions, and reducing agents or photocatalytic reactions are mostly used. Complex and economically unreasonable.

Method used

The red mud is separated by a low-concentration hydrochloric acid-oxalic acid two-stage leaching acid leaching process, combined with ascorbic acid or sodium ascorbate as reducing agent, and redox reaction and chemical precipitation are used to prepare ferrous oxalate and iron hydroxide colloid.

Benefits of technology

It realizes efficient preparation of ferrous oxalate, reduces acid consumption, improves environmental friendliness, simplifies the process flow, and improves the quality and economicality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115466174B_ABST
    Figure CN115466174B_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently utilizing red mud to prepare ferrous oxalate. The method combines redox reaction and chemical precipitation equilibrium principle, adopts a low-concentration hydrochloric acid-oxalic acid two-stage acid leaching process for leaching treatment, and performs graded separation and directional conversion on an iron-containing solution to prepare ferrous oxalate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental pollution control, and in particular to a method for efficiently preparing ferrous oxalate by utilizing red mud. Background Art

[0002] Red mud is an industrial solid waste residue produced in the process of producing alumina by alkali dissolution or alkali roasting of bauxite. It has the characteristics of high alkali and high salt. Large-scale storage poses huge hidden dangers and environmental hazards to soil, water and atmosphere. Red mud contains a large number of iron-containing minerals, whose mineral particles are small and are mutually cemented and embedded, making it difficult to effectively separate, resulting in poor resource utilization. At present, the technologies for recovering iron from red mud are mainly divided into physical methods (magnetic separation, gravity separation, etc.), chemical methods (acid leaching, roasting, etc.), and biological methods. The physical method of iron extraction is simple and low in cost, but the recovery rate is not high and the product quality is poor; the fire reduction process in the chemical method is relatively mature and has a high recovery rate, but the process is complicated and prone to secondary pollution; wet acid leaching has low energy consumption, but there are problems such as co-existence and leaching of impurity ions; the biological method is environmentally friendly, but there are problems such as long time consumption. Invention patent CN102674643A discloses a method for leaching iron oxide from red mud by oxalic acid and photocatalysis. The patent uses 0.5-1 mol / L oxalic acid solution as the leaching agent, and the solid-liquid ratio of air-dried red mud to oxalic acid solution is 80-120 g / L. Stirring at 60-90°C for 30-240 min, a photochemical reaction occurs under ultraviolet light or sunlight to form ferrous oxalate precipitation. Invention patent CN103922416A discloses a method for separating and recovering iron from red mud, wherein iron in red mud is removed by leaching with oxalic acid solution, and iron-removed red mud and a leachate containing ferrous oxalate are obtained by filtration. The obtained iron-removed red mud is used as a raw material for producing cement and refractory bricks. The obtained ferric oxalate-containing leachate is subjected to membrane electrolysis or adding a reducing agent (iron powder or iron filings) to reduce the ferric oxalate therein to ferrous oxalate for precipitation, or directly adding one or more of calcium oxide, calcium hydroxide, and calcium carbonate to obtain a mixed precipitate of calcium oxalate and ferric hydroxide. The ferrous oxalate precipitate or the mixed precipitate of calcium oxalate and ferric hydroxide is decomposed by acid to recover oxalic acid and obtain an iron-containing product.

[0003] At present, the patents for recycling iron from red mud that have been disclosed have problems such as high consumption of inorganic acid, environmental unfriendliness, and coexistence of impurity ions. The present invention adopts a two-stage graded acid leaching process of hydrochloric acid and oxalic acid to carry out directional separation of red mud. Ferrous oxalate can be used as a raw material for lithium iron phosphate, a new type of battery material, and its application value is higher. In the iron-containing oxalic acid solution leached with oxalic acid in the existing patents, iron is Fe 2+ and Fe 3+In the past, ferric oxalate appeared in the form of ions, and the ferric oxalate was reduced to ferrous oxalate precipitate by adding a reducing agent (iron powder or iron filings) or photocatalytic reaction, which was economically unreasonable and complicated in technical route. In this regard, the patent uses readily available ascorbic acid or sodium ascorbate solution as a reducing agent, and uses a spiral flow microchannel reaction system to accelerate mass transfer and make the reaction effect better. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing ferrous oxalate by efficiently utilizing red mud, which realizes the combination of redox reaction and chemical precipitation equilibrium principle, adopts a low-concentration hydrochloric acid-oxalic acid two-stage acid leaching process for leaching treatment, and performs graded separation and directional conversion on the iron-containing solution to prepare ferrous oxalate and ferric hydroxide colloid.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for efficiently utilizing red mud to prepare ferrous oxalate is carried out according to the following steps:

[0007] (1) drying the red mud in an oven, grinding it, and pulverizing it through a 40-60 mesh sieve;

[0008] (2) adding a low concentration hydrochloric acid solution to the red mud, placing the mixture in a magnetic stirrer for mixing and stirring for 1 to 2 hours, and then filtering under reduced pressure, placing the obtained filter residue in an electric heated blast drying oven for 1 to 2 hours to a constant weight, and obtaining dealkalized red mud;

[0009] (3) mixing the treated dealkalized red mud with the oxalic acid solution and placing the mixture in a water bath constant temperature oscillator, heating the mixture in a water bath for reaction, and filtering the mixture while hot to obtain a second-stage iron-containing oxalic acid filtrate;

[0010] (4) Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump. The two injection tube outlets are connected together through a T-shaped three-way pipe so that the fluids in the injection tubes A and B can converge into a flow stream to assemble a mixed flow system. A micro silicone tube with a length of 1 to 1.5 m is connected to the T-shaped tube outlet, and the silicone tube is tightly wound around a round tube with a diameter of 1 to 2 cm to form a spiral flow microchannel; the flow rate is adjusted to allow it to react fully.

[0011] Further; in step (2), the concentration of the low concentration hydrochloric acid solution is C HCl ≦1mol·L -1 .

[0012] Further, in step (3), the treated dealkalized red mud is treated at a solid-liquid ratio of 1:3 to 15 g·mL -1 With a concentration of 1 to 4 mol·L -1The oxalic acid solution was mixed and placed in a water bath constant temperature oscillator.

[0013] Further, in step (3), the reaction is carried out by heating in a water bath at 90-95°C for 1-2 hours.

[0014] Furthermore, in step (4), the microchannel reaction system adjusts the flow rate so that the single flow rate is 0.5 to 5 mL / min.

[0015] Further, in step (3), the concentrations of ascorbic acid and sodium ascorbate solution are 0.02 to 0.1 mol·L -1 .

[0016] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0017] 1. In view of the problems of high acid consumption, environmental unfriendliness, and coexistence of impurity ions in the current acid leaching process using inorganic acids, this experiment introduces oxalic acid as the acid leaching medium and uses a two-stage graded acid leaching process of hydrochloric acid-oxalic acid to separate red mud. Compared with inorganic acids, oxalic acid is less toxic and dangerous, and is a biodegradable and environmentally friendly acid. It has been used in metal leaching to a certain extent. In this experiment, it is used as an acid leaching agent to transfer the mineral iron phase in the solid phase to the liquid phase to achieve directional conversion and efficiently prepare ferrous oxalate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is the reaction flow chart of the present invention.

[0019] Figure 2 This is the XRD pattern of the red mud of the present invention.

[0020] Figure 3 This is a SEM image of the red mud of the present invention.

[0021] Figure 4 This is the XRD before and after dealkalization of the red mud of the present invention.

[0022] Figure 5 This is the XRD of the original red mud sample and the red mud residue after two-stage oxalic acid leaching of the present invention.

[0023] Figure 6 The infrared spectrum of the preparation of ferrous oxalate of the present invention.

[0024] Figure 7 The figure is the XRD spectrum of ferrous oxalate prepared according to the present invention.

[0025] Figure 8 It is the change of the iron content in the solution under the reducing conditions of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0027] Example 1

[0028] A method for efficiently preparing ferrous oxalate using red mud,

[0029] Proceed as follows:

[0030] (1) drying the red mud in an oven, grinding it, and pulverizing it through a 40-mesh sieve;

[0031] (2) adding a low concentration hydrochloric acid solution to the red mud, placing the mixture in a magnetic stirrer for mixing and stirring for 1 hour, and then filtering under reduced pressure, placing the obtained filter residue in an electric heated blast drying oven and drying it for 1 hour to constant weight, thereby obtaining dealkalized red mud;

[0032] (3) mixing the treated dealkalized red mud with the oxalic acid solution and placing the mixture in a water bath constant temperature oscillator, heating the mixture in a water bath for reaction, and filtering the mixture while hot to obtain a second-stage iron-containing oxalic acid filtrate;

[0033] (4) Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump, and the two injection tube outlets are connected together through a T-shaped three-way pipe so that the fluids in the injection tubes A and B can converge into a flow stream to assemble a mixed flow system, and a micro silicone tube with a length of 1 m is connected to the T-shaped tube outlet, and the silicone tube is tightly wound around a round tube with a diameter of 1 cm to form a spiral flow microchannel; the flow rate is adjusted to allow it to react fully;

[0034] In step (2), the concentration of the low concentration hydrochloric acid solution is C HCl ≦1mol·L -1 ;

[0035] In step (3), the treated dealkalized red mud is mixed with water at a solid-liquid ratio of 1:15 g·mL -1 With a concentration of 1 mol·L -1 The oxalic acid solution was mixed and placed in a water bath constant temperature oscillator;

[0036] In step (3), the reaction was carried out in a water bath at 90° C. for 2 h;

[0037] In step (4), the flow rate of the microchannel reaction system is adjusted so that the single-branch flow rate is 0.5 mL / min;

[0038] In step (3), the concentrations of ascorbic acid and sodium ascorbate solution are both 0.02 mol·L -1; It is convenient to prepare ferrous oxalate using red mud.

[0039] Example 2

[0040] A method for efficiently utilizing red mud to prepare ferrous oxalate is carried out according to the following steps:

[0041] (1) drying the red mud in an oven, grinding it, and pulverizing it through a 50-mesh sieve;

[0042] (2) adding a low concentration hydrochloric acid solution to the red mud, placing the mixture in a magnetic stirrer for mixing and stirring for 1.5 hours, and then filtering under reduced pressure. The resulting filter residue was placed in an electric heated blast drying oven and dried for 1.5 hours to constant weight to obtain dealkalized red mud;

[0043] (3) mixing the treated dealkalized red mud with the oxalic acid solution and placing the mixture in a water bath constant temperature oscillator, heating the mixture in a water bath for reaction, and filtering the mixture while hot to obtain a second-stage iron-containing oxalic acid filtrate;

[0044] (4) Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump, and the two injection tube outlets are connected together through a T-shaped three-way pipe so that the fluids in the injection tubes A and B can converge into a flow stream to assemble a mixed flow system, and a micro silicone tube with a length of 1.25 m is connected to the T-shaped tube outlet, and the silicone tube is tightly wound around a round tube with a diameter of 1.5 cm to form a spiral flow microchannel; the flow rate is adjusted to allow it to react fully;

[0045] In step (2), the concentration of the low concentration hydrochloric acid solution is C HCl ≦1mol·L -1 ;

[0046] In step (3), the treated dealkalized red mud is mixed with water at a solid-liquid ratio of 1:3 g·mL -1 With a concentration of 2.5 mol·L -1 The oxalic acid solution was mixed and placed in a water bath constant temperature oscillator;

[0047] In step (3), the reaction was carried out at 92.55° C. in a water bath for 1.5 h;

[0048] In step (4), the flow rate of the microchannel reaction system is adjusted so that the single-branch flow rate is 3 mL / min;

[0049] In step (3), the concentrations of ascorbic acid and sodium ascorbate solutions are both 0.06 mol·L -1 . It is convenient to prepare ferrous oxalate using red mud.

[0050] Example 3

[0051] A method for efficiently utilizing red mud to prepare ferrous oxalate is carried out according to the following steps:

[0052] (1) drying the red mud in an oven, grinding it, and pulverizing it through a 60-mesh sieve;

[0053] (2) adding a low concentration hydrochloric acid solution to the red mud, placing the mixture in a magnetic stirrer for mixing and stirring for 2 hours, and then filtering under reduced pressure, placing the resulting filter residue in an electric heated blast drying oven for 2 hours to a constant weight, and obtaining dealkalized red mud;

[0054] (3) mixing the treated dealkalized red mud with the oxalic acid solution and placing the mixture in a water bath constant temperature oscillator, heating the mixture in a water bath for reaction, and filtering the mixture while hot to obtain a second-stage iron-containing oxalic acid filtrate;

[0055] (4) Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump, and the two injection tube outlets are connected together through a T-shaped three-way pipe so that the fluids in the injection tubes A and B can converge into a flow stream to assemble a mixed flow system, and a 1.5 m long micro silicone tube is connected to the T-shaped tube outlet, and the silicone tube is tightly wound around a round tube with a diameter of 2 cm to form a spiral flow microchannel; the flow rate is adjusted to allow it to react fully;

[0056] In the step (2), the concentration of the low concentration hydrochloric acid solution is C HCl ≦1mol·L -1 ;

[0057] In step (3), the treated dealkalized red mud is mixed with water at a solid-liquid ratio of 1:9 g·mL -1 With a concentration of 4 mol·L -1 The oxalic acid solution was mixed and placed in a water bath constant temperature oscillator;

[0058] In step (3), the reaction was carried out in a water bath at 95° C. for 1 h;

[0059] In step (4), the flow rate of the microchannel reaction system is adjusted so that the single-branch flow rate is 5 mL / min;

[0060] In step (3), the concentrations of ascorbic acid and sodium ascorbate solutions are both 0.1 mol·L -1 . It is convenient to prepare ferrous oxalate using red mud.

[0061] Experimental procedures

[0062] Red mud dealkalization pretreatment

[0063] (1) The red mud was placed in an oven for drying, ground, and passed through a 40-mesh sieve before the experiment was carried out.

[0064] (2) Add 5 g red mud and 30 mL 1 mol·L -1 The HCl solution was placed in a magnetic stirrer and stirred for 1 hour, then filtered, and the obtained filter residue was placed in an electric heated blast drying oven and dried for 1 hour to obtain the dealkalized red mud.

[0065] Second stage oxalic acid leaching

[0066] Add dealkalized red mud and oxalic acid solution (21 g of oxalic acid solid dissolved in 70 mL of distilled water) into a 100 mL beaker, place in a water bath constant temperature oscillator, heat in a water bath to 363 K for 2 h, filter while hot to obtain the second-stage oxalic acid filtrate.

[0067] Preparation of ferrous oxalate

[0068] Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump. The two injection tube outlets are connected together through a T-type three-way pipe so that the fluids in injection tubes A and B can converge into a stream and assemble into a mixed flow system. A micro silicone tube with a length of 1 to 1.5 m is connected to the T-type tube outlet, and the silicone tube is tightly wound on a round tube with a diameter of 1 to 2 cm to form a spiral microchannel; the flow rate is adjusted to make it fully reacted. After the crystals are completely precipitated, they are filtered to obtain ferrous oxalate. Dry, weigh, and calculate its yield.

[0069] After the red mud has been de-alkaliized by hydrochloric acid pretreatment, oxalic acid solution is added to allow iron to enter the solution in the form of ions, and a reducing agent is added to precipitate through redox reaction and chemical reaction, so that oxalate ions combine with ferrous ions to produce yellow ferrous oxalate precipitate. sp (FeC2O4) = 3.2 × 10 -7 , K sp (Fe(OH)3)=4.0×10 -38 .

[0070] Fe2O3+3H2C2O4·2H2O=Fe2(C2O4)3+9H2O

[0071]

[0072] Fe 3+ + Reductant → Fe 2+

[0073]

[0074] In the experiment, the main oxides of red mud components are shown in Table 1. Figure 1The size of the spiral flow microchannel is at the micron level. By utilizing the advantages of efficient heat transfer and easy control of reaction conditions (reactant ratio, temperature, pressure, reaction time and flow rate, etc.) of the microchannel reactor, the materials in the spiral flow microchannel can be fully mixed quickly in a short time. Figure 2 From the XRD spectrum analysis, it can be seen that the main phase in red mud is Fe2O3. Figure 3 SEM results show that red mud is composed of particles of different sizes and distributed in a layered and blocky manner, which confirms that the mineral particles are small and are cemented and embedded with each other, making it difficult to effectively separate them. Figure 4 , Figure 5 The XRD phase analysis of the filter residues from the two acid leachings showed that the characteristic peak of Fe2O3 had basically disappeared, and by comparing the XRD standard cards of ferrous oxalate and ferric hydroxide, no ferrous oxalate and ferric hydroxide crystals were found in the filter residues. Figure 6 , 7 , 8, the infrared spectrum shows that 3300cm -1 The broad peak at 1619 cm is the absorption peak of crystal water. -1 The strong peak at 820 cm is due to the vibration of the carboxyl C=O. -1 The peak at the wavelength is the bending vibration absorption peak of OCO, 700cm -1 The following two peaks are the stretching vibration absorption peaks of Fe-O. The angle and intensity of the diffraction peaks in the XRD spectrum are consistent with the standard card of ferrous oxalate, so the three reducing agents can prepare ferrous oxalate. The change of iron content in the solution under different reduction conditions ( Figure 8 ) It can be seen that when ascorbic acid is used as a reducing agent, the iron ion content in the solution decreases rapidly and reaches equilibrium, taking into account the ease of operation of the experiment. The reduction system formed by the addition of ascorbic acid is more effective for the preparation of ferrous oxalate, and the time for producing ferrous oxalate is shorter and the yield is higher.

[0075] Table 1 Main oxides of red mud components

[0076]

[0077] Although the present invention is described herein with reference to a number of illustrative embodiments of the present invention, it will be appreciated that those skilled in the art may devise many other modifications and implementations that fall within the scope and spirit of the principles disclosed herein. More specifically, within the scope of the present disclosure, drawings, and claims, a variety of variations and modifications may be made to the components and / or layout of the subject combination layout. In addition to the variations and modifications made to the components and / or layout, other uses will also be apparent to those skilled in the art.

Claims

1. A method for preparing ferrous oxalate using red mud, Features: Proceed as follows: (1) Dry the red mud in an oven, grind it, and pulverize it through a 40-60 mesh sieve; (2) Adding a low concentration hydrochloric acid solution to the red mud, placing the mixture in a magnetic stirrer for 1 to 2 hours, and then filtering under reduced pressure. The resulting filter residue is placed in an electric heated blast drying oven and dried for 1 to 2 hours to a constant weight to obtain dealkalized red mud; (3) mixing the treated dealkalized red mud with the oxalic acid solution and placing it in a water bath constant temperature oscillator, heating it in a water bath for reaction, and filtering it while hot to obtain a second-stage iron-containing oxalic acid filtrate; (4) Ascorbic acid, sodium ascorbate solution and second-stage oxalic acid leaching solution are placed in injection tube A and injection tube B respectively, and installed on the injection pump. The two injection tube outlets are connected together through a T-shaped three-way pipe so that the fluids in injection tubes A and B can converge into one flow to assemble a mixed flow system. A micro silicone tube with a length of 1 to 1.5 m is connected to the T-shaped tube outlet, and the silicone tube is tightly wound around a round tube with a diameter of 1 to 2 cm to form a spiral flow microchannel; the flow rate is adjusted to allow it to react fully; In the step (3), the treated dealkalized red mud is mixed with water at a solid-liquid ratio of 1:3-15 g·mL -1 With a concentration of 1~4 mol·L -1 The oxalic acid solution was mixed and placed in a water bath constant temperature oscillator; In step (3), the water bath is heated at 90-95 o C for 1-2 hours; In the step (4), the microchannel reaction system adjusts the flow rate so that the single-branch flow rate is 0.5-5 mL / min; In step (3), the concentrations of ascorbic acid and sodium ascorbate solution are both 0.02-0.10 mol·L -1 ; In the step (2), the concentration of the low concentration hydrochloric acid solution is C HCl ≦1mol·L -1 .

Citation Information

Patent Citations

  • Method for recovering ferric oxide from red mud by leaching-photocatalysis by oxalic acid

    CN102674643A

  • Method for separating and recovering iron from red mud

    CN103922416A

  • Method for synthesizing strip-shaped ferrous oxalate from hematite slag in one pot

    CN114105759A

  • Method for preparing ferrous oxalate from siderite

    CN114560767A

  • Magnetite production from bauxite residue

    US20190177178A1