A hyperbranched acrylate composition and light-cured acrylate pressure-sensitive adhesive and preparation method thereof

Synthesizing the hyperbranched acrylate composition by a two-step method has solved the problems of insufficient performance and environmental pollution of the photocured acrylate pressure-sensitive adhesive in the prior art, and achieved the preparation of green and environmentally friendly pressure-sensitive adhesives with high peel strength and low energy consumption.

CN115477723BActive Publication Date: 2024-11-08JINAN NORTH TAIHE NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211177752.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-26
Publication Date
2024-11-08
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

It is difficult to prepare photocured acrylate pressure-sensitive adhesives with high peel strength and high light transmission properties in the prior art, and the use of a large amount of solvents during the traditional preparation process leads to environmental pollution and high energy consumption.

Method used

The hyperbranched acrylate composition was synthesized by two-step method, and linear acrylic resin was prepared by free radical polymerization, and then a starting agent and a catalyst were added for heating reaction to form a hyperbranched structural acrylate composition for preparation of solvent-free photocured acrylic acid Ester pressure sensitive glue.

Benefits of technology

A green and environmentally friendly chemical process without solvents and no waste was achieved, and a new superbranched structured acrylate pressure-sensitive adhesive with high peel strength, high light transmission and high weather resistance was prepared.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the field of adhesive materials, and particularly relates to a hyperbranched acrylate composition, a light-curing acrylate pressure-sensitive adhesive and a preparation method thereof. The hyperbranched acrylate composition is synthesized by a two-step method. A linear acrylic resin containing two functional groups, a hydroxyl group and an epoxy group, is first prepared by free radical polymerization. Then, an initiator and a catalyst are added, and the temperature is raised to gradually polymerize the hydroxyl group and the epoxy group to synthesize the hyperbranched acrylate composition. The light-curing acrylate pressure-sensitive adhesive is prepared by using the composition as a raw material. The whole reaction process is solvent-free and does not generate three wastes. The reaction is in line with the concept of green environmental protection chemical industry and belongs to an environmentally friendly new material. The obtained novel hyperbranched acrylate pressure-sensitive adhesive has the properties of high peel strength, high light transmittance, high weather resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesive materials, and in particular relates to a hyperbranched acrylate composition and a light-curing acrylate pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] Acrylic pressure-sensitive adhesives are widely used in the fields of machinery, automobiles, electronics, packaging, and consumption, and are the most widely used adhesive types. Traditional acrylic pressure-sensitive adhesives are mostly solvent-based or emulsion-based: solvent-based ones pollute the environment and affect the health of production personnel, and the use of a large amount of solvents has the risk of flammability and explosion during production and transportation; emulsion-based ones have the disadvantages of high energy consumption and poor water resistance. Photocuring technology has the characteristics of high efficiency, energy saving, and environmental protection. Photocuring acrylic pressure-sensitive adhesives not only retain the weather resistance, high transparency, wide bonding, and low cost advantages of acrylic adhesive systems, but also realize the system without solvents, 100% solid content, and rapid curing, achieving the concept of green, environmental protection, energy saving, and health throughout the life cycle of adhesives. There have been many studies on photocuring acrylic pressure-sensitive adhesives, but most of them are thermally initiated or photoinitiated acrylic monomers that form linear acrylic resins through free radical polymerization, or synthesize polyurethane acrylate prepolymers, and then compound photocrosslinkers, photoinitiators, etc. to prepare acrylic pressure-sensitive adhesives. Whether it is a linear acrylate resin or a polyurethane acrylate prepolymer, when the molecular weight is low, the pressure-sensitive adhesive can easily infiltrate the substrate and has good spreadability, but the low cohesive energy leads to low peel strength; when the molecular weight is high, the bulk strength of the pressure-sensitive adhesive is significantly improved, but the viscosity will also increase significantly, which is not conducive to infiltrating the substrate. High-viscosity adhesives are also not easy to coat into films, and the initial viscosity of the pressure-sensitive adhesive will decrease. Generally, a small amount of solvent (high solid content), water-based or hot-melt type is used to reduce the viscosity of the pressure-sensitive adhesive through different methods such as solvent, water or temperature, which is conducive to the coating of the pressure-sensitive adhesive into a film. However, it will bring environmental pollution and high energy consumption, weakening the original advantages of light-curing acrylic pressure-sensitive adhesives.

[0003] Hyperbranched structural materials have a topological structure that is completely different from traditional linear molecules. They have highly branched structures, a large number of end groups, and weak intermolecular entanglement. Therefore, their physical and chemical properties are very unique, and they have shown superior performance advantages in the fields of coatings and adhesives. Under the same molecular weight, hyperbranched structural resins have significantly lower viscosity, and the branched structure has more active sites (groups) that interact with the substrate, so this technology can be used to obtain photocurable acrylic pressure-sensitive adhesives with better performance.

[0004] There are many reports on hyperbranched acrylate materials in the existing literature. The hyperbranched poly (ester-amine) described in patent CN107652443A is prepared by the Michael addition reaction of acrylate groups and amine groups. The hyperbranched molecule ends with a large number of acrylate groups, and contains hydroxyl groups or hydroxyl groups and alkenyl groups coexisting inside. However, the preparation process is cumbersome, requiring the use of a large amount of solvents (methanol, dimethyl sulfoxide, ether and petroleum ether) and the recovery of ethylenediamine raw materials by distillation. The unreacted amine groups are easily oxidized during the rotary evaporation process, and the product color becomes darker, and the energy consumption is large. The use of a large amount of organic solvents is very likely to cause solvent volatilization to pollute the environment and there are potential safety hazards such as flammable and explosive. The hyperbranched acrylate resin prepared by patent CN112321842A is also obtained by the Michael addition reaction of acrylate groups and amine groups to obtain a hyperbranched acrylate resin capped with acrylate groups, but the molecular weight and functionality of this hyperbranched structure mainly depend on the number of active hydrogens of the polyamine, and have the characteristics of low molecular weight, high functionality, and high photocuring activity, which is suitable for preparing high hardness ultraviolet light-cured products. The two acrylate-terminated hyperbranched materials above are not pressure-sensitive after photocuring and are not suitable for the preparation of pressure-sensitive adhesives.

[0005] Therefore, whether it is possible to obtain a light-cured acrylic pressure-sensitive adhesive with better performance has become one of the problems to be solved urgently in this field. Summary of the invention

[0006] The present invention aims at the many deficiencies in the prior art, provides a hyperbranched acrylate composition and a light-cured acrylate pressure-sensitive adhesive and a preparation method thereof, wherein the hyperbranched acrylate composition is synthesized by a two-step method, wherein a linear acrylic resin containing two functional groups, hydroxyl and epoxy, is first prepared by free radical polymerization, and then an initiator and a catalyst are added, and the temperature is raised to gradually polymerize the hydroxyl and epoxy groups to synthesize the hyperbranched acrylate composition; and the light-cured acrylate pressure-sensitive adhesive is prepared by using the composition as a raw material. The whole reaction process is solvent-free and does not generate three wastes, which conforms to the concept of green environmental protection chemical industry and belongs to an environmentally friendly new material. The obtained hyperbranched structure novel acrylate pressure-sensitive adhesive has the properties of high peel strength, high light transmittance, high weather resistance and the like.

[0007] The invention firstly provides a hyperbranched acrylate composition. Specifically, the hyperbranched acrylate composition is synthesized by a two-step method. Firstly, a linear acrylic resin is prepared by free radical polymerization. The linear acrylic resin contains two functional groups, hydroxyl and epoxy. Then, an initiator and a catalyst are added. The temperature is increased to gradually polymerize the hydroxyl and epoxy groups to synthesize the hyperbranched acrylate composition.

[0008] The specific preparation steps are as follows:

[0009] Step 1: Add acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan into a three-necked flask, pass nitrogen protection, start stirring, and then slowly heat to 56°C to 60°C, keep warm and react for 5 hours to obtain a linear acrylic resin;

[0010] The mass ratio of acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan is 99-99.5:0.1-0.3:0.4-0.6;

[0011] The preferred mass ratio of acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan is 99.4:0.1:0.5;

[0012] The second step: adding a catalyst accounting for 0.8% of the total weight of the linear acrylic resin to the linear acrylic resin obtained in the first step, adding a secondary amine monomer as an initiator at a ratio of 1 / 26 to 1 / 8 of the molar number of epoxy groups in the reaction system, adding a diluent at a ratio of 60% of the total mass of the linear acrylic resin, adding an inhibitor at a ratio of 0.05% to 0.8% of the total mass of the linear acrylic resin, and then heating to 100° C. to 110° C., reacting for 3 hours, to obtain a hyperbranched acrylate composition.

[0013] The catalyst is selected from one of p-toluenesulfonic acid, benzyltriethylammonium chloride or triphenylphosphine;

[0014] The acrylic ester monomers are composed of glycidyl methacrylate and hydroxyl-containing monomers, as well as soft monomers, hard monomers and polar monomers; and the amount of glycidyl methacrylate does not exceed 2% of the total weight of the acrylic ester monomers; and the molar ratio of the total hydroxyl group to the epoxy group in all monomers is 2-4:1.

[0015] Furthermore, the hydroxyl-containing monomer is selected from one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxy-terminated caprolactone acrylate, and hydroxyethyl acrylamide;

[0016] The soft monomer is 2-ethylhexyl acrylate or / and butyl acrylate;

[0017] The hard monomer is isobornyl acrylate and / or methyl methacrylate;

[0018] The polar monomer is selected from one or more of acryloylmorpholine, acrylonitrile, N,N-dimethylacrylamide and N,N-diethylacrylamide.

[0019] Most preferably, the composition of the multiple acrylic acid ester monomers is as follows by weight: 2-4 parts of glycidyl methacrylate, 4-16 parts of hydroxyl-containing monomers, 8-16 parts of hard monomers, 2-8 parts of polar monomers, and 56-84 parts of soft monomers. At this time, it is still necessary to control the amount of glycidyl methacrylate to not exceed 2% of the total weight of the acrylic acid ester monomers; at the same time, the total molar ratio of hydroxyl groups to epoxy groups in all monomers is 2-4:1, otherwise the second step reaction is likely to form gel.

[0020] The secondary amine monomer is selected from but not limited to polyaspartic acid ester, Jefflink 136 and Jefflink 754 of Huntsman Company, Clearlink 1000 and Clearlink 3000 of Dorf Ketal Company, and can be one of them or a mixture of several;

[0021] Polyaspartic acid ester is a sterically hindered bifunctional secondary amine monomer, which is specifically purchased from Shenzhen Feiyang Junyan New Materials Co., Ltd. in this application. The available brands are F520, F420, F2850, F2872, F221, etc.

[0022] The diluent is selected from but not limited to 2-ethylhexyl acrylate; the inhibitor includes but is not limited to p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol.

[0023] In the above reaction process, the linear acrylic resin obtained in the first step contains hydroxyl and epoxy functional groups, and the molar ratio of hydroxyl to epoxy groups is maintained at 2 to 4:1. A trace amount of secondary amine is used as an initiator to react with the epoxy group, and then a hyperbranched acrylic resin is obtained through an iterative reaction of hydroxyl and epoxy groups.

[0024] For better understanding, the inventors assume that the total molar ratio of hydroxyl groups to epoxy groups in all monomers is 3:1, and polyaspartic acid ester is used as a representative of secondary amines. The specific schematic formula (1 iteration) of the second step reaction process is as follows:

[0025]

[0026] In the above examples, R may represent an alkyl moiety containing 1 to 20 carbon atoms, preferably 3 to 12 carbon atoms, the alkyl group may be linear or branched; or a cycloalkyl group containing 6 to 15 carbon atoms;

[0027] Preferred alkyl and cycloalkyl moieties include, for example, 1,4-butyl, 1,6-hexyl, 2,2,4-trimethylhexyl, 3,3,5-trimethylcyclohexane, dicyclohexylmethane;

[0028] R' may represent an alkyl group containing 1 to 6 carbon atoms, preferably a methyl group and / or an ethyl group.

[0029] After one iteration, the polymer has 6 branches and 18 terminal hydroxyl groups; if the reaction reaches the second iteration, the hyperbranched structure is more complex, with 18 branches and 54 terminal hydroxyl groups. And so on, but the more iterations, the polymer molecular weight increases significantly, the viscosity also increases significantly, which is not conducive to the stability of the reaction, and it is easy to have a side reaction between the secondary hydroxyl group and the epoxy group, resulting in gelation. Therefore, the number of iterations is controlled by controlling the amount of secondary amine monomer added, and then the polymer viscosity is controlled.

[0030] Therefore, the inventors have determined that the molar number of the secondary amine monomer is 1 / 26 to 1 / 8 of the total molar number of epoxy groups, and more preferably 1 / 16 to 1 / 8, and the number of iterations does not exceed 2 times; when the proportion is lower than 1 / 26, the final molecular weight is too high, the viscosity increases, and gelation is easily caused by side reactions during the reaction. In addition, too high a viscosity is not conducive to the wetting of the substrate and construction of the pressure-sensitive adhesive; when it is higher than 1 / 8, sufficient branches cannot be generated, the hyperbranched structure is incomplete, and the characteristics of the hyperbranched structure cannot be brought into play.

[0031] Adding a small amount of polar monomers during copolymerization can increase intramolecular or intermolecular hydrogen bonds, significantly improve the cohesive force of the pressure-sensitive adhesive, and improve the adhesion and peel strength to polar substrates. The polar monomers selected in the present invention are all alkaline substances, do not contain acidic components, will not corrode ITO (indium tin oxide) layers, metal layers and other bonding substrates, and can be used in the field of high-end electronics.

[0032] The hyperbranched acrylate composition obtained by the above method has the following characteristics:

[0033] The invention is a hyperbranched acrylic ester composition obtained by further reaction with a linear acrylic resin as a raw material, wherein the side chains are all long molecular chains (linear acrylic resin), and each side chain is very flexible, which is conducive to sufficient wetting of a substrate, improving initial adhesion and elongation, and is different from the short-chain structure hyperbranched polymer obtained by the reaction of small molecules in the past; the multifunctional terminal hydroxyl groups are easy to establish hydrogen bonds with polar substrates, etc., thereby improving peel strength. Therefore, the pressure-sensitive adhesive prepared with the hyperbranched acrylic ester composition synthesized by the invention as a raw material has both high peel strength and high elongation, which is a key performance that is highly valued in the pressure-sensitive adhesive for laminating flexible electronic screens.

[0034] The photocurable acrylate pressure-sensitive adhesive prepared by using the above-synthesized hyperbranched acrylate composition as raw material has the following components in mass percentage: 35% to 68.8% of the hyperbranched acrylate composition, 30% to 60% of the acrylate monomer diluent, 0.2% to 1% of the antioxidant, and 1% to 4% of the photoinitiator;

[0035] The acrylic acid ester monomer diluent is composed of 2-ethylhexyl acrylate, hydroxyethyl acrylate and isobornyl acrylate, wherein the mass ratio of each component is: 1 to 4 parts of 2-ethylhexyl acrylate, 1 to 4 parts of hydroxyethyl acrylate, and 2 to 6 parts of isobornyl acrylate;

[0036] The antioxidant is one or more of antioxidant 245 (triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate), antioxidant 1076 (β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), and antioxidant 1135 (3,5-di-tert-butyl-4-hydroxyphenylpropionate).

[0037] The photoinitiator is a combination of one or more of benzoin dimethyl ether, benzophenone, 1-hydroxycyclohexyl phenyl ketone (abbreviated as: 184 photoinitiator), 2-hydroxy-2-methyl-1-phenyl-1-propanone (abbreviated as: 1173 photoinitiator), 2-methyl-1-(4-methylthio)phenyl-2-morpholinylpropyl-1-one (IRGACURE 907), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (abbreviated as: TPO photoinitiator), 2,4,6-trimethylbenzoylphosphonic acid ethyl ester phenyl (abbreviated as: TPO-L photoinitiator), and bis(2,4,6-trimethylbenzoyl)phosphine oxide (IRGACURE 819);

[0038] The preparation method of the above-mentioned light-curing acrylate pressure-sensitive adhesive is as follows:

[0039] At room temperature, add the acrylate monomer diluent into the container according to the above mass percentage, then add the photoinitiator and the antioxidant, stir until the photoinitiator and the antioxidant are dissolved and mixed evenly, then add the hyperbranched acrylate composition, stir evenly, and the entire preparation process is carried out in the dark (or under yellow light) to avoid the photoinitiator initiating polymerization, resulting in increased viscosity or gel.

[0040] The photocurable pressure-sensitive adhesive prepared with the hyperbranched acrylate composition can be used for self-supporting OCA adhesive film (for 3C product electronic screen bonding), high peel strength double-sided pressure-sensitive tape, high-performance weather-resistant and heat-resistant pressure-sensitive adhesive (such as automotive, home appliances and other fields).

[0041] The innovation of the present invention is that a novel hyperbranched acrylate composition is synthesized by a two-step method, and a light-cured acrylate pressure-sensitive adhesive is prepared by using the composition as a raw material. The whole reaction process is solvent-free and does not produce three wastes, which conforms to the concept of green environmental protection chemical industry and belongs to an environmentally friendly new material. The obtained hyperbranched structure novel acrylate pressure-sensitive adhesive has high peel strength, high light transmittance, high weather resistance and other properties. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with the embodiments, which may enable those skilled in the art to more fully understand the present invention, but does not limit the present invention in any way;

[0043] Embodiment 1:

[0044] A hyperbranched acrylate composition, wherein the preparation method of the hyperbranched acrylate composition is:

[0045] Step 1: Add various acrylic acid ester monomers, dibenzoyl peroxide, and dodecyl mercaptan into a three-necked flask, pass nitrogen protection, start stirring at 100-300 rpm, then slowly heat to 56°C-60°C, keep warm and react for 5 hours to obtain a linear acrylic resin;

[0046] The mass percentage ratio of each raw material component in the first step reaction is: 99.4% of various acrylate monomers, 0.1% of dibenzoyl peroxide and 0.5% of dodecyl mercaptan;

[0047] The above-mentioned multiple acrylic acid ester monomers are composed of the following components in the following mass proportions: 2 parts of glycidyl methacrylate, 3 parts of hydroxypropyl methacrylate, 3 parts of hydroxyethyl acrylate, 16 parts of isobornyl acrylate, 6 parts of acryloylmorpholine, and 70 parts of 2-ethylhexyl acrylate; wherein the molar ratio of the total amount of hydroxyl groups of the hydroxyl-containing monomers to the total amount of epoxy groups of glycidyl methacrylate is 3:1;

[0048] Step 2: adding triphenylphosphine catalyst, an appropriate amount of F420 secondary amine monomer as an initiator, 2-ethylhexyl acrylate as a diluent, and an appropriate amount of 2,6-di-tert-butyl-p-cresol as a polymerization inhibitor to the linear acrylic resin obtained in the first step, and then heating to 100° C. to 110° C. and reacting for 3 hours to obtain a hyperbranched acrylic ester composition;

[0049] The mass percentage ratio of each raw material component in the second step reaction is: linear acrylic resin 77%, 2-ethylhexyl acrylate 21.2%, triphenylphosphine 0.6%, 2,6-di-tert-butyl-p-cresol 0.8%, F420 secondary amine 0.4%.

[0050] The technical scheme for preparing a light-curing acrylate pressure-sensitive adhesive using the above-synthesized hyperbranched acrylate composition as a raw material is as follows:

[0051] The mass percentage ratio of the components of the light-curing acrylic pressure-sensitive adhesive is: 60% of the hyperbranched acrylic composition, 38.5% of the acrylic monomer diluent, 0.5% of the antioxidant 245, and 1% of the photoinitiator TPO.

[0052] Further, the acrylic acid ester monomer diluent is composed of the following components in the following mass ratios: 2 parts of 2-ethylhexyl acrylate, 1.5 parts of hydroxyethyl acrylate, and 5 parts of isobornyl acrylate;

[0053] The preparation method of the light-curing acrylic pressure-sensitive adhesive is as follows: first, add an acrylic acid ester monomer diluent into a container, then add a photoinitiator and an antioxidant, stir until the photoinitiator and the antioxidant are dissolved and mixed evenly, then add a hyperbranched acrylic acid ester composition, stir evenly, filter and remove impurities to obtain a light-curing acrylic pressure-sensitive adhesive. All materials must be used at room temperature or heated to no more than 60° C., and the entire preparation process is carried out in the dark (or under yellow light) to avoid the photoinitiator initiating polymerization to cause viscosity increase or gelation.

[0054] Example 2

[0055] The main experimental steps are the same as those in Example 1, with the following changes:

[0056] The mass percentage ratio of each raw material component in the second step reaction is: linear acrylic resin 77%, 2-ethylhexyl acrylate 21.4%, triphenylphosphine 0.6%, 2,6-di-tert-butyl-p-cresol 0.8%, F420 secondary amine 0.2%.

[0057] Example 3

[0058] The main experimental steps are the same as those in Example 1, with the following changes:

[0059] The mass percentage ratio of each raw material component in the second step reaction is: linear acrylic resin 77%, 2-ethylhexyl acrylate 21.5%, triphenylphosphine 0.6%, 2,6-di-tert-butyl-p-cresol 0.8%, F420 secondary amine 0.1%.

[0060] Example 4

[0061] In the first step of synthesizing the hyperbranched acrylate composition, the addition ratio of acryloylmorpholine was changed from 6 parts to 4 parts, and the rest was the same as in Example 1.

[0062] Example 5

[0063] In the first step of synthesizing the hyperbranched acrylate composition, the addition ratio of acryloylmorpholine was changed from 6 parts to 2 parts, and the rest was the same as in Example 1.

[0064] Example 6

[0065] In the first step of synthesizing the hyperbranched acrylate composition, the addition ratio of acryloylmorpholine was changed from 6 parts to 8 parts, and the rest was the same as in Example 1.

[0066] Comparative Example 1

[0067] Referring to Example 1 of patent CN109810648A on a UV-curable non-woven tape and a preparation method thereof, a UV-curable acrylate coating liquid was prepared and tested.

[0068] Comparative Example 2

[0069] An acrylic emulsion pressure-sensitive adhesive was prepared with reference to Example 1 of patent CN104497201A, and the performance was tested.

[0070] Product performance testing

[0071] The adhesive products of each embodiment were coated on a PET (75 μm thick) film using a flat coater to control the film thickness to 80 μm, and then covered with a PET release film, placed under a 150-watt UV-LED lamp for irradiation for 1 minute (the main wavelength is 395 nm), and the release film was removed to obtain a pressure-sensitive tape, which was tested according to the standards. The 180° peel strength and adhesion time were measured according to GB / T 2792-2014 and GB / T 4851-2014 standards, respectively, and the viscosity and transmittance were measured according to GB / T 2794-2013 and GB / T 2410-2008 standards, respectively. The failure type refers to the failure type of the 180° peel strength, which can be divided into: interface failure and cohesive failure.

[0072] The adhesive products of Examples 1 to 6 were respectively used for bonding performance tests, and the results are shown in the following table:

[0073]

[0074] Comparing the test results, it can be seen from Examples 1, 2, and 3 that as the secondary amine content of the initiator gradually decreases, the viscosity of the prepared light-cured acrylate pressure-sensitive adhesive gradually increases, and the 180° peel strength also tends to increase. The reduction in the secondary amine content of the initiator leads to an increase in the number of iterations of the hyperbranched structure, an increase in the molecular weight, and enhanced cohesion, which is beneficial to improving the bonding strength. However, when the viscosity is too high, it will affect the wetting effect of the adhesive on the substrate, resulting in unsatisfactory bonding strength.

[0075] Comparing Examples 5, 4, 1, and 6, the addition ratio of the polar monomer acryloylmorpholine was gradually increased by 2 parts, 4 parts, 6 parts, and 8 parts, respectively, and the 180° peel strength gradually increased from 15N / 25mm to 34 N / 25mm. It can be seen that the increase in the content of polar monomers in the synthesis of the hyperbranched acrylate composition will significantly increase the peel strength of the pressure-sensitive adhesive. Comprehensively considering various performance performances, the product prepared in Example 6 has a lower viscosity, is conducive to construction and coating, has the largest 180° peel strength, and has the best performance.

[0076] The damage types of the examples are all interface damage, indicating that the cohesive strength of the pressure-sensitive adhesive is higher than the interface bonding strength. Compared with the linear acrylic resin used in the traditional pressure-sensitive adhesive, the hyperbranched acrylic resin used in the examples of the present invention has the characteristics of high cohesive strength, so it shows interface damage. At the same time, the light transmittance of the light-curing acrylic pressure-sensitive adhesive is greater than 90%, which is suitable for optical applications, such as electronic screen bonding.

[0077] In comparative example 1, acrylate glue is directly used to coat a film 80 μm thick. After UV curing, the 180° peel strength is only 18N / 25mm, and the damage form is interface + cohesive damage. Because the molecular structure is a linear structure, the cohesion of the adhesive layer is low, and there are small molecular weight acrylate oligomers, which leads to reduced bonding performance. Small molecular weight acrylate oligomers are easy to remain on the bonding substrate, and its viscosity is 5000 mPa S, which is much higher than the viscosity range of the embodiments of the present application, and it is not easy to coat.

[0078] Comparative Example 2 has a lower viscosity, but it is a water-based pressure-sensitive adhesive and requires a drying process after coating, which is energy-consuming and complex in process. In addition, the 180° peel strength is only 9.1 N / 25 mm, which is much lower than the 180° peel strength of 15 to 34 N / 25 mm of the present application.

[0079] It can be seen that the technical solution of the present application is significantly better than the prior art.

[0080] In summary, in the technical solution of the present invention, the bonding strength can be improved by reducing the content of secondary amine initiator or increasing the proportion of polar monomers in the hyperbranched acrylate composition within a certain range during the preparation of the photocurable acrylate pressure-sensitive adhesive.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A hyperbranched acrylate composition, characterized in that: First, a linear acrylic resin is prepared by free radical polymerization, and then an initiator and a catalyst are added, and the temperature is raised to gradually polymerize the hydroxyl group and the epoxy group to obtain the resin. The specific preparation method has the following steps: Step 1: Add acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan into a three-necked flask, pass nitrogen protection, start stirring, and then slowly heat to 56°C to 60°C, keep warm and react for 5 hours to obtain a linear acrylic resin; The mass ratio of acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan is 99-99.5:0.1-0.3:0.4-0.6; Step 2: adding a catalyst accounting for 0.8% of the total weight of the linear acrylic resin to the linear acrylic resin obtained in the first step, adding a secondary amine monomer as an initiator at a ratio of 1 / 26 to 1 / 8 of the molar number of epoxy groups in the reaction system, adding a diluent at a ratio of 60% of the total weight of the linear acrylic resin, adding a polymerization inhibitor at a ratio of 0.05% to 0.8% of the total weight of the linear acrylic resin, and then heating to 100° C. to 110° C. and reacting for 3 hours to obtain a hyperbranched acrylate composition; The catalyst is selected from one of p-toluenesulfonic acid, benzyltriethylammonium chloride or triphenylphosphine; The secondary amine monomer is selected from one or a mixture of polyaspartic acid ester, Jefflink136 and Jefflink754 of Huntsman Company, Clearlink 1000 and Clearlink 3000 of Dorf Ketal Company; the diluent is selected from 2-ethylhexyl acrylate; the inhibitor includes one of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol; the molar ratio of the total hydroxyl group to the epoxy group in all the acrylate monomers is 2 to 4:

1.

2. The method for preparing the hyperbranched acrylate composition according to claim 1, characterized in that: The specific preparation steps are as follows: Step 1: Add acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan into a three-necked flask, pass nitrogen protection, start stirring, and then slowly heat to 56°C to 60°C, keep warm and react for 5 hours to obtain a linear acrylic resin; The mass ratio of acrylate monomer, dibenzoyl peroxide and dodecyl mercaptan is 99-99.5:0.1-0.3:0.4-0.6; Step 2: adding a catalyst accounting for 0.8% of the total weight of the linear acrylic resin to the linear acrylic resin obtained in the first step, adding a secondary amine monomer as an initiator at a ratio of 1 / 26 to 1 / 8 of the molar number of epoxy groups in the reaction system, adding a diluent at a ratio of 60% of the total weight of the linear acrylic resin, adding a polymerization inhibitor at a ratio of 0.05% to 0.8% of the total weight of the linear acrylic resin, and then heating to 100° C. to 110° C. and reacting for 3 hours to obtain a hyperbranched acrylate composition; The catalyst is selected from one of p-toluenesulfonic acid, benzyltriethylammonium chloride or triphenylphosphine; The secondary amine monomer is selected from one or a mixture of polyaspartic acid ester, Jefflink136 and Jefflink754 of Huntsman Company, Clearlink 1000 and Clearlink 3000 of Dorf Ketal Company; the diluent is selected from 2-ethylhexyl acrylate; the inhibitor includes one of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol; the molar ratio of the total hydroxyl group to the epoxy group in all the acrylate monomers is 2 to 4:

1.

3. The method for preparing a hyperbranched acrylate composition according to claim 2, wherein: The acrylate monomer is composed of glycidyl methacrylate and a hydroxyl-containing monomer, as well as a soft monomer, a hard monomer, and a polar monomer, and the mass ratio of the acrylate monomer, dibenzoyl peroxide, and dodecyl mercaptan is 99.4:0.1:0.5; The polar monomer is selected from one or more of acryloylmorpholine, acrylonitrile, N,N-dimethylacrylamide and N,N-diethylacrylamide.

4. The method for preparing a hyperbranched acrylate composition according to claim 3, wherein: The hydroxyl-containing monomer is selected from one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxy-terminated caprolactone acrylate, and hydroxyethyl acrylamide; The soft monomer is 2-ethylhexyl acrylate or / and butyl acrylate; The hard monomer is isobornyl acrylate and / or methyl methacrylate.

5. The method for preparing a hyperbranched acrylate composition according to claim 4, wherein: The acrylic acid ester monomer composition is as follows by weight: 2-4 parts of glycidyl methacrylate, 4-16 parts of hydroxyl-containing monomer, 8-16 parts of hard monomer, 2-8 parts of polar monomer, 56-84 parts of soft monomer; and the amount of glycidyl methacrylate does not exceed 2% of the total weight of the acrylic acid ester monomer.

6. The method for preparing the hyperbranched acrylate composition according to claim 5, characterized in that: The molar ratio of the total amount of hydroxyl groups in the hydroxyl-containing monomer to the total amount of epoxy groups in glycidyl methacrylate is 2 to 4:

1.

7. A light-curable acrylate pressure-sensitive adhesive containing the hyperbranched acrylate composition according to claim 1, characterized in that: The mass percentage of each component is: 35% to 68.8% of the hyperbranched acrylate composition, 30% to 60% of the acrylate monomer diluent, 0.2% to 1% of the antioxidant, and 1% to 4% of the photoinitiator.

8. The light-curing acrylate pressure-sensitive adhesive according to claim 7, characterized in that: The acrylic acid ester monomer diluent is composed of 2-ethylhexyl acrylate, hydroxyethyl acrylate and isobornyl acrylate, wherein the mass ratio of each component is: 1 to 4 parts of 2-ethylhexyl acrylate, 1 to 4 parts of hydroxyethyl acrylate, and 2 to 6 parts of isobornyl acrylate; The antioxidant is one or more of antioxidant 245, antioxidant 1076, and antioxidant 1135; The photoinitiator is a combination of one or more of benzoin dimethyl ether, benzophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.

9. The method for preparing the light-curing acrylate pressure-sensitive adhesive according to claim 7, characterized in that: The specific steps are: Adding an acrylate monomer diluent into the container according to the above mass percentage, then adding a photoinitiator and an antioxidant, stirring until the photoinitiator and the antioxidant are dissolved and mixed evenly, then adding a hyperbranched acrylate composition, stirring evenly, filtering to remove impurities to obtain a light-cured acrylate pressure-sensitive adhesive; All materials must be used at room temperature or heated to no more than 60°C, and the entire preparation process must be carried out in the dark or under yellow light.