Polyarylspirobifluorene and its application in organic electroluminescent devices

By using polyaryl spirobifluorene compounds as the main material of organic electroluminescent devices, the HOMO/LUMO and triple-twisted energy levels are solved, and the energy level matching problem of main material in the prior art is improved, and the luminescence efficiency and device life are improved. , and provides new synthesis ideas for all carbon skeleton materials, achieving efficient and stable photoelectric performance.

CN115490568BInactive Publication Date: 2024-11-12SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110682942.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-18
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The synthesis of main materials in existing organic electroluminescent devices is difficult to achieve high-efficiency energy level matching, resulting in low luminescence efficiency, short device life, and insufficient design flexibility.

Method used

1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene, 1,3,3 ,6,8-tetraaryl spirobifluorene and other polyaryl spirobifluorene compounds are used as main materials. Through the design of specific substituent structures, HOMO/LUMO energy levels and triplet energy levels are formulated, and a variety of luminescent materials are suitable for use in a variety of luminescent materials. , improve exciton utilization and reduce efficiency roll-off.

Benefits of technology

It has achieved good photoelectric properties and thermal stability of polyaryl spirobifluorene compounds, and is suitable for blue, green and red phosphorescent OLEDs, which improves device efficiency, reduces efficiency roll-off, and provides full carbon skeleton body materials. The new synthesis idea has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115490568B_ABST
    Figure CN115490568B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of organic electroluminescent materials, and in particular to a novel structure of 1,3-diaryl spirobifluorene, 1,6-diaryl spirobifluorene, 1,3,6-triaryl spirobifluorene, 1,3,7-triaryl spirobifluorene, 1,3,6,8-tetraaryl spirobifluorene and the application of the material in an organic electroluminescent display device. The structural formula of the 1,3-diaryl spirobifluorene, 1,6-diaryl spirobifluorene, 1,3,6-triaryl spirobifluorene, 1,3,7-triaryl spirobifluorene and 1,3,6,8-tetraaryl spirobifluorene derivatives is as shown in Formula I: #imgabs0# The present invention provides a method for preparing a polyaryl spirobifluorene electroluminescent host material molecule and the application of the polyaryl spirobifluorene as a host material in making an organic electroluminescent device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of spirobifluorene derivatives, and specifically relates to the structures, preparation methods and applications of 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene and 1,3,6,8-tetraarylspirobifluorene. Background Art

[0002] Organic light-emitting diodes (OLEDs) have been a new technology in the field of display and lighting and have always attracted much attention from academia and industry. Since Deng Qingyun and others prepared the first organic electroluminescent device in 1987, the structure and efficiency of OLED devices have been greatly innovated and improved. Doping devices, that is, dispersing luminescent molecules in the main material, can avoid the concentration quenching effect of the luminescent material to improve the luminous efficiency of the device, and can also slow down the aging process of the device to increase the life of the device. In addition, the use of doped luminescence can also increase the flexibility of device design, thereby making the application prospects of luminescent materials broader.

[0003] In recent years, research on host materials in organic electroluminescent devices is in the ascendant. The host materials in OLED devices must have good carrier transport performance and can form pinhole-free films. Considering the characteristics of the luminescent materials and device structure, the host materials must have the following properties: 1. The HOMO / LUMO energy level of the dopant material is embedded in the host material. 2. The emission spectrum of the host material has an effective overlap with the absorption spectrum of the dopant material. 3. The host material has a higher triplet energy level to prevent the reverse transfer of triplet energy from the dopant material to the host material. 4. The positive and negative carrier transport in the host material needs to be balanced to limit the exciton recombination area to the device light-emitting layer. 5. The HOMO / LUMO energy level of the host material matches the energy level of the adjacent hole transport layer and electron transport layer to reduce the injection barrier and reduce the device startup voltage. Therefore, the synthesis of energy level matching and high-efficiency host materials faces challenges. Summary of the invention

[0004] The purpose of the present invention is to provide a series of novel main materials with 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene and 1,3,6,8-tetraarylspirobifluorene structures as the central skeleton.

[0005] The 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene, and 1,3,6,8-tetraarylspirobifluorene compounds of the present invention have a structure shown in Formula I:

[0006]

[0007] Wherein, Ar represents any one of a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted heteroaryl group having 1 to 30 carbon atoms, a substituted or unsubstituted arylamine group having 6 to 30 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkylsilyl group having 6 to 30 carbon atoms, a nitro group, a cyano group, and a halogen group.

[0008] Preferably, the organic electroluminescent host material includes but is not limited to the following structural formula:

[0009]

[0010]

[0011]

[0012] The second object of the present invention is to provide a method for preparing the above-mentioned organic electroluminescent host material, and the reaction formula is as follows:

[0013]

[0014] The third object of the present invention is to provide an organic electroluminescent host material based on 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene, and 1,3,6,8-tetraarylspirobifluorene as a main material of the light-emitting layer, and its application in the field of manufacturing organic electroluminescent devices.

[0015] The present invention includes but is not limited to the following 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene, 1,3,7-triarylspirobifluorene, 1,3,6,8-tetraarylspirobifluorene structures:

[0016]

[0017]

[0018] The substituents R are the same or different and are independently selected from hydrogen, deuterium, substituted or unsubstituted alkyl having 1 to 30 carbon atoms, substituted or unsubstituted alkenyl having 2 to 24 carbon atoms, substituted or unsubstituted alkynyl having 2 to 24 carbon atoms, substituted or unsubstituted aryl having 6 to 30 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 30 carbon atoms, substituted or unsubstituted heterocycloalkyl having 1 to 30 carbon atoms, substituted or unsubstituted heteroaryl having 1 to 30 carbon atoms, substituted or unsubstituted any one of an alkoxy group having 1 to 30 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, a substituted or unsubstituted alkylthio group having 1 to 30 carbon atoms, a substituted or unsubstituted arylthio group having 6 to 30 carbon atoms, a substituted or unsubstituted alkylamino group having 1 to 30 carbon atoms, a substituted or unsubstituted arylamino group having 6 to 30 carbon atoms, a substituted or unsubstituted alkylsilyl group having 1 to 30 carbon atoms, a substituted or unsubstituted arylsilyl group having 6 to 30 carbon atoms, a nitro group, a cyano group and a halogen group.

[0019] The prepared organic electroluminescent device includes an ITO conductive glass substrate (anode), a hole injection layer (HAT-CN), a hole transport layer (TAPC), an electron blocking layer (TCTA, mCP), a light-emitting layer (FIrPic doped in the organic electroluminescent host material of the present invention), an electron transport layer (TmPyPB), an electron injection (LiF), and a cathode layer (Al) stacked in sequence. The organic electroluminescent device is prepared by vacuum evaporation. The molecular structures of some organic compounds used in the device are as follows.

[0020]

[0021] The beneficial effects of the present invention are:

[0022] 1. The polyaryl spirobifluorene compounds provided by the present invention have good photoelectric properties and thermal stability, and the HOMO and LUMO energy levels are easy to adjust, so they are suitable for a variety of luminescent materials, can improve the utilization rate of excitons, reduce efficiency roll-off, and have good photoelectric properties.

[0023] 2. The 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene and 1,3,6,8-tetraarylspirobifluorene provided by the present invention can be used as the main material of blue phosphorescent OLEDs due to their high triplet energy levels; 1,3-diarylspirobifluorene, 1,6-diarylspirobifluorene, 1,3,6-triarylspirobifluorene and 1,3,6,8-tetraarylspirobifluorene can also be used as the main material of green phosphorescent OLEDs; 1,3,7-triarylspirobifluorene can be used as the main material to sensitize red phosphorescent materials.

[0024] 3. The main material produced by the present invention can be used to sensitize thermally activated delayed fluorescence (TADF) materials for the production of OLED devices, and has good device performance, achieves high efficiency, and reduces efficiency roll-off, and has good prospects for industrial application.

[0025] 4. The polyaryl spirobifluorene prepared by the present invention has great application potential in all-carbon skeleton main materials, and provides a new synthesis idea for this type of all-carbon skeleton main materials, which also shows the superiority of C-H activation as a synthesis strategy in the development of optoelectronic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 H NMR spectrum of compound 3.

[0027] Figure 2 Compound 3 NMR spectrum C

[0028] Figure 3 H NMR spectrum of compound B4.

[0029] Figure 4 NMR spectrum of compound B4 C spectrum.

[0030] Figure 5 Single crystal structure of compound B1.

[0031] Figure 6 Single crystal structure of compound B2.

[0032] Figure 7 Single crystal structure of compound B3.

[0033] Figure 8 A schematic structural diagram of an organic electroluminescent device according to the present invention. DETAILED DESCRIPTION

[0034] In order to better understand the content of the present invention, the present invention is explained below in conjunction with specific examples, which are not intended to limit the scope of the present invention.

[0035] Example 1: Preparation of Compound B4

[0036]

[0037] Under nitrogen atmosphere, [Cp*IrCl2]2 (3.9 mg, 2.5 mol%), AgSbF6 (6.9 mg, 10 mol%), Ag2O (92.7 mg, 2.0 equiv.), PivOH (20.4 mg, 1.0 equiv.), p-phenylbenzoic acid (1, 0.2 mmol), diaryliodonium salt (2, 0.42 mmol) and DCE (1.0 mL) were added to a Schlenk tube with a magnetic stirrer. The resulting mixture was stirred at 120-150°C for 12-24 hours and then diluted with 5 mL of CH2Cl2. The solution was filtered through a diatomaceous earth pad and washed with 10-25 mL of CH2Cl2. The filtrate was concentrated in vacuo and the residue was purified by silica gel column chromatography (petroleum ether / CH2Cl2=4 / 1, v / v) to provide the desired product 3. 1 H NMR (400MHz, CDCl3): δ=7.87(s,1H),7.78-7.67(m,11H),7.65-7.61(m,2H),7.54-7.45(m,8H),7.39(t,J=7.2Hz,2H)ppm. 13 C NMR (100MHz, CDCl3): δ=192.53,147.38,146.24,142.51,142.28,142.08,141.17,140.82,139.90,139.84,136.37,135.50,132.99,130.30 ,129.68,129.00,128.93,128.80,128.78,128.61,127.89,127.38,127.23,127.20,126.82,126.70,122.66,120.38,118.08ppm.HRMS (ESI + ): Calculated value C 37 H 25 O[M+H] + 485.1900, measured value: 485.1905. The H NMR spectrum of 3 is shown in the attached Figure 1 , see the attached NMR carbon spectrum Figure 2 .

[0038]

[0039] Under nitrogen atmosphere, 2-bromobiphenyl (1.1 equivalents), 40 mL of anhydrous tetrahydrofuran were added to a Schlenk tube with a magnetic stirrer and cooled to -78°C, followed by slow dripping of 1.0 equivalents of 2.5 mol / L n-butyl lithium solution. The reaction system was stirred at -78°C for one hour and then slowly dripped 1.0 equivalents of reactant 3 dissolved in 20 mL of anhydrous tetrahydrofuran. The reaction system was then heated to 75°C and stirred for 24 hours. After the reaction was completed, it was cooled to room temperature and quenched with a dilute ammonium chloride solution. The reaction system was extracted with ethyl acetate and dried with anhydrous sodium sulfate. After removing the solvent, 100 mL of 1,2-dichloroethane was used to dissolve the remaining solid and 5.0 equivalents of boron trifluoride ether solution were slowly added. The reaction system was stirred at room temperature for three hours and then quenched with methanol, and the solvent was removed. The residue was purified by silica gel column chromatography (petroleum ether / CH2Cl2=8 / 1, v / v) to provide the desired product 4. 1 H NMR (400MHz, CDCl3): δ = 8.13 (s, 1H), 8.01 (d, J = 8.0Hz, 1H), 7.75 (d, J = 7.6Hz, 2H), 7.65 (d, J = 8.0Hz, 1H), 7.52-7.44 (m, 6H), 7. 43-7.34(m,6H),7.32-7.26(m,3H),7.22(t,J=7.4Hz,3H),7.09(t,J=7.6Hz,2H),6.91-6.85(m,5H),6.23(d,J=8.4Hz,2H)ppm. 13 C NMR (100MHz, CDCl3): δ=150.14,148.12,145.37,142.66,142.17,141.47,141.1 1,140.97,140.87,140.84,140.53,140.46,138.55,137.60,128.83,128.66,12 8.63,128.53,128.21,127.44,127.31,127.25,127.12,127.03,127.02,126.98 ,126.76,125.29,123.97,122.58,120.31,119.78,117.59,65.61ppm.HRMS(ESI + ): Calculated value C 49 H 33 [M+H] + 621.2577, measured value: 621.2577. See the attached H NMR spectrum of B4. Figure 3 , see the attached NMR carbon spectrum Figure 4 .

[0040] Example 2-4: The preparation of compounds B1, B2, and B3 is based on Example 1. The single crystal structure of B1 is shown in the attached Figure 5 The single crystal structure of B2 is shown in the attached Figure 6 The single crystal structure of B3 is shown in the attached Figure 7 .

[0041] Application examples of organic electroluminescent devices:

[0042] The present invention uses compounds B1, B2, B3, B4 and commercially available 4,4'-bis(9H-carbazole-9-yl)biphenyl (CBP) as the main material to prepare the organic electroluminescent device, and uses commercially available phosphorescent or thermally activated delayed fluorescent materials as the luminescent material. Figure 8 As shown, the organic electroluminescent device comprises, from bottom to top, an ITO conductive glass substrate (1), a hole injection layer (2), a hole transport layer (3), a light emitting layer (4), an electron transport layer (5), an electron injection layer (6), and a cathode layer (7). It should be understood that the device implementation process and results are only for better explanation of the present invention, and are not intended to limit the present invention.

[0043]

[0044] Application Example 1

[0045] The phosphorescent organic electroluminescent device was prepared as follows:

[0046] 1. Cleaning ITO (indium tin oxide) glass: wash with alkali and deionized water in sequence, dry in a vacuum drying oven, and then treat in a plasma cleaner for 10 minutes;

[0047] 2. On the anode ITO glass, vacuum evaporate the hole injection layer HAT-CN (10 nm), the hole transport layer TAPC (30 nm), the electron blocking layer TCTA (10 nm), and the exciton blocking layer mCP (10 nm) in sequence, with an evaporation rate of 0.1 nm / s;

[0048] 3. Vacuum evaporate the light-emitting layer on the electron blocking layer, (3%) Ir(mphmp)2tmd:B4, the evaporation rate is 0.1nm / s, and the evaporation thickness is 20nm;

[0049] 4. Vacuum evaporate the electron transport layer TmPyPb (40 nm) on the light-emitting layer at a rate of 0.1 nm / s;

[0050] 5. Vacuum evaporate the electron injection layer LiF (0.8 nm) on the electron transport layer at a rate of 0.08 nm / s;

[0051] 6. Vacuum evaporate cathode Al (100 nm) on the electron injection layer at a rate of 0.1 nm / s.

[0052] The device structures used include:

[0053] Blue light: ITO / HAT-CN (10nm) / TAPC (30nm) / TCTA (10nm) / mCP (10nm) / B1:15wt%Flrpic, (20nm) / TmPyPB (50nm) / LiF (0.8nm) / Al (100nm);

[0054] ITO / HAT-CN(10nm) / TAPC(30nm) / TCTA(10nm) / mCP(10nm) / B2:15wt%Flrpic,(20nm) / TmPyPB(40nm) / LiF(0.8nm) / Al(100nm).

[0055] Green light: ITO / HAT-CN (10nm) / TAPC (30nm) / TCTA (10nm) / B2:15wt%Ir(ppy)3, (20nm) / TmPyPB (60nm) / LiF (0.8nm) / Al (100nm);

[0056] ITO / HAT-CN(10nm) / TAPC(30nm) / TCTA(10nm) / B3:15wt%Ir(ppy)3,(20nm) / TmPyPB(50nm) / LiF(0.8nm) / Al(100nm);

[0057] ITO / HAT-CN(10nm) / TAPC(30nm) / TCTA(10nm) / B4:15wt%Ir(ppy)3,(20nm) / TmPyPB(40nm) / LiF(0.8nm) / Al(100nm).

[0058] Red light: ITO / HAT-CN (10nm) / TAPC (30nm) / TCTA (10nm) / mCP (10nm) / B3: 3wt% Ir(mphmp)2tmd, (20nm) / TmPyPB (40nm) / LiF (0.8nm) / Al (100nm);

[0059] ITO / HAT-CN(10nm) / TAPC(30nm) / TCTA(10nm) / mCP(10nm) / B4:3wt%Ir(mphmp)2tmd,(20nm) / TmPyPB(40nm) / LiF(0.8nm) / Al(100nm);

[0060] ITO / HAT-CN(10nm) / TAPC(30nm) / TCTA(10nm) / mCP(10nm) / CBP:3wt%Ir(mphmp)2tmd,(20nm) / TmPyPB(40nm) / LiF(0.8nm) / Al(100nm).

[0061] Comparative Example

[0062] An organic electroluminescent device was prepared according to the method of Application Example 1, except that compound CBP was used instead of compound B4 as the luminescent material. The test results of the obtained device are shown in Table I.

[0063] Using compound B4 as the main material of the device, the test results of the obtained device are shown in Table I.

[0064] Table I

[0065]

[0066] For comparison, the present invention manufactures CBP as a reference device. As shown in Table I, the device current efficiency based on CBP is 29.9 lm / W, and the maximum EQE is 19.2%. The organic electroluminescent device prepared based on the material of the present invention exhibits good device performance, with a maximum power efficiency of 44.4 lm / W and a maximum EQE of 27.3%. Compared with the comparative device CBP, the device exhibits excellent characteristics in terms of current efficiency and device efficiency.

[0067] The performance test results of devices 2 to 7 prepared in Application Examples 2-7 are shown in Table II.

[0068] Table II

[0069]

[0070]

[0071] Application Example 2

[0072] The thermally activated delayed fluorescence organic electroluminescent device was prepared as follows:

[0073] 1. Cleaning ITO (indium tin oxide) glass: wash with alkali and deionized water in sequence, dry in a vacuum drying oven, and then treat in a plasma cleaner for 10 minutes;

[0074] 2. On the anode ITO glass, vacuum evaporate the hole injection layer HAT-CN (10nm) and the hole transport layer α-NPD (60nm) in sequence, with an evaporation rate of 0.1nm / s;

[0075] 3. Vacuum evaporate the light-emitting layer on the electron blocking layer, (8%) B1:4CzIPN, the evaporation rate is 0.1nm / s, and the evaporation thickness is 30nm;

[0076] 4. Vacuum evaporate the hole blocking layer mBPDBT (5nm) and the electron transport layer ZADN (40nm) on the light-emitting layer at a rate of 0.1nm / s;

[0077] 5. An electron injection layer Liq (2 nm) was vacuum-deposited on the electron transport layer at a rate of 0.08 nm / s; 6. A cathode Al (120 nm) was vacuum-deposited on the electron injection layer at a rate of 0.1 nm / s.

[0078] The device structure is: ITO / HAT-CN (10nm) / α-NPD (60nm) / B4:4CzIPN (8wt%, 30nm) / mBPDBT (5nm) / ZADN (40nm) / Liq (2nm) / Al (120nm).

[0079] The above descriptions are only some implementation cases of the present invention and are not intended to limit the present invention. Any modifications, substitutions, etc. made within the spirit and principles of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a polyaryl spirobifluorene electroluminescent host material molecule, characterized in that: The following steps are involved: 1) wherein Ar represents an unsubstituted aryl group having 6 to 30 carbon atoms; 2) under nitrogen atmosphere, [Cp*IrCl2]2, AgSbF6, Ag2O, PivOH, benzoic acid derivative (1), diaryliodonium salt (2) and DCE were added to a Schlenk tube equipped with a magnetic stirrer, and the resulting mixture was stirred at 80-150°C for 6-48 hours. After the reaction was completed, it was cooled to room temperature and then diluted with CH2Cl2. The solution was filtered through diatomaceous earth and washed with CH2Cl2. The filtrate was concentrated in vacuo and the residue was purified by silica gel column chromatography to provide the desired product 3; 3) Under nitrogen atmosphere, 2-bromobiphenyl and anhydrous tetrahydrofuran were added to a Schlenk tube with a magnetic stirrer and cooled to -78°C, followed by slow dripping of 1.0 equivalent of butyl lithium solution. After the reaction system was stirred at -78°C for one hour, 1.0 equivalent of reactant 3 dissolved in anhydrous tetrahydrofuran was slowly dripped, and then the reaction system was heated to 50-100°C and stirred for 24 hours. After the reaction was completed, it was cooled to room temperature and quenched with a dilute ammonium chloride solution. The reaction system was extracted with ethyl acetate and dried with anhydrous sodium sulfate. After removing the solvent, the remaining solid was dissolved with 1,2-dichloroethane and 5.0 equivalents of boron trifluoride ether solution were slowly added. The reaction system was stirred at room temperature for three hours. After the reaction was completed, methanol was added to quench and the solvent was removed. The residue was purified by silica gel column chromatography to provide the desired product 4.