Low dielectric constant hypercrosslinked polymer / polyimide composite film for high frequency, preparation method and application

The preparation of hypercrosslinked polymer/polyimide composite films by blending hypercrosslinked polymers with polyamic acid solutions solves the problem of high dielectric constant in traditional polyimide films at high frequencies, achieving a balance between low dielectric constant, high thermal stability, and mechanical strength.

CN115505151BActive Publication Date: 2024-11-05ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211238918.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-09
Publication Date
2024-11-05
Estimated Expiration
2042-10-09

AI Technical Summary

Technical Problem

Traditional polyimide films have a high dielectric constant at high frequencies, making it difficult to meet the requirements for low dielectric constants. Furthermore, they suffer from severe dielectric loss at high frequencies. In addition, the introduction of inorganic fillers can easily cause interface problems, making it difficult to balance high frequency, low dielectric constant, high temperature resistance, and mechanical properties.

Method used

A hypercrosslinked polymer/polyimide composite film was prepared by physical blending of hypercrosslinked polymer and polyamic acid solution through an amidation reaction. The microporous structure and high specific surface area of ​​the hypercrosslinked polymer were utilized to reduce the dielectric constant of the composite film while maintaining excellent thermal stability and mechanical strength.

Benefits of technology

It achieves an extremely low dielectric constant at high frequencies while maintaining good thermal stability and mechanical strength. The dielectric constant decreases to 1.6-2.5 in the range of 8.2-12.4 GHz, the thermal stability T5% is 453℃, and the tensile strength and modulus are 92 MPa and 2.15 GPa, respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003879948140000011
    Figure HDA0003879948140000011
  • Figure HDA0003879948140000012
    Figure HDA0003879948140000012
  • Figure HDA0003879948140000021
    Figure HDA0003879948140000021
Patent Text Reader

Abstract

The present invention provides a hyper-crosslinked polymer / polyimide composite film with low dielectric constant under high-frequency working conditions, a preparation method and application thereof. The present invention mixes diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and aprotic solvent, performs polymerization reaction to generate polyamic acid, adds hyper-crosslinked polymer, and then performs step-by-step temperature amidation treatment to obtain a polyimide composite film; the mass content of the hyper-crosslinked polymer in the composite film is 5% to 20%. The present invention adds hyper-crosslinked polymer during the reaction process, so that the hyper-crosslinked polymer is more evenly dispersed in the composite film, and the addition amount of the hyper-crosslinked polymer is controlled, so that the dielectric constant of the composite film under high-frequency working conditions can be reduced, while maintaining good thermal stability and mechanical properties. The prepared composite film can be used in the fields of integrated circuits, microelectronics and insulating materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymers, and in particular to a low dielectric constant hypercrosslinked polymer / polyimide composite film for high frequency use, a preparation method and an application thereof. Background Art

[0002] Polyimide (PI) is a high-performance polymer material obtained by the condensation reaction of dibasic anhydride and diamine, and its molecular chain is composed of repeating units containing imide rings. Among them, aromatic polyimide has higher heat resistance, mechanical strength and chemical stability, because its molecular chain repeating unit has the conjugation effect of aromatic heterocycles and nitrogen-containing five-membered heterocycles, and electron transfer complexation can be formed within and between molecules. The application of polyimide in the field of microelectronics mainly includes the following aspects: interlayer insulation materials, photosensitive polyimide and flexible printed circuit boards. Traditional PI film has excellent electrical insulation, heat resistance, low dielectric constant (about 3.5, 10 3 Hz) and corrosion resistance, it is the main insulating substrate for current flexible printed circuit boards. However, due to the increase in 5G communication frequency, insulating films with low dielectric constants (less than 3) or even ultra-low dielectric constants (less than 2.2) are essential to ensure high-speed, low-latency and low-loss transmission of electromagnetic signals. The higher dielectric constant of traditional PI films makes it difficult to meet the above (ultra) low dielectric constant requirements, and its dielectric loss is serious in the high-frequency band. Therefore, it is necessary to develop a low dielectric constant and high-temperature resistant PI suitable for high-frequency bands.

[0003] In order to reduce the dielectric properties of PI, groups are often introduced to reduce the overall polarity of the polymer, or inorganic fillers with low dielectric constants are added to PI to reduce the dielectric constant of PI. However, the effect of introducing group modification to reduce the dielectric constant in the high frequency band is often not significant enough; and the introduction of inorganic fillers is often prone to interface problems due to the structural differences between inorganic and organic materials. Although there are also reports on some other modifications, they often cannot take into account high frequency, low dielectric constant, high temperature resistance and mechanical properties. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a polyimide composite film, preparation method and application thereof for high-frequency working conditions, which utilizes the microporous structure, high specific surface area and spatial effect of the hyper-crosslinked polymer itself to reduce the dielectric constant of the composite film. Using diamine monomer and dianhydride monomer as raw materials, a precursor polyamic acid is prepared, and the hyper-crosslinked polymer and the precursor polyamic acid are evenly mixed by physical blending to prepare a polyamic acid composite solution containing the hyper-crosslinked polymer, and then the temperature is stepped to perform an amidation reaction, which has the characteristics of short reaction cycle, simple and efficient processing method, and large-scale production. The polyimide composite film prepared by the present invention has an extremely low dielectric constant under high-frequency working conditions, and takes into account excellent thermal stability and mechanical strength.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a hyper-crosslinked polymer / polyimide composite film with a low dielectric constant at high frequencies, the specific steps of which are:

[0007] (1) blending diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and a non-protonic solvent by physical blending method, and performing polymerization reaction to obtain a precursor polyamic acid;

[0008] (2) adding a hyper-crosslinked polymer to a precursor polyamic acid solution, and physically blending the mixture to obtain a polyamic acid composite solution containing the hyper-crosslinked polymer;

[0009] (3) The polyamic acid composite solution containing the hyper-crosslinked polymer is coated on a glass plate and the temperature is increased stepwise to carry out an amidation reaction, and then the solution is peeled off from the glass plate and dried to obtain a low dielectric constant hyper-crosslinked polymer / polyimide composite film for high frequency use.

[0010] Preferably, the mass ratio of the diaminodiphenyl ether to hexafluoroisopropylene diphthalic anhydride is 1:(2.3-2.5).

[0011] Preferably, the solvent includes one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

[0012] Preferably, the ratio of the diaminodiphenyl ether to the solvent is 1 g: (9-10) mL.

[0013] Preferably, the polymerization reaction temperature is -5 to 5°C, the subsequent polymerization temperature is room temperature, and the polymerization reaction time is 6 to 8 hours.

[0014] Preferably, the mass content of the hyper-crosslinked polymer in the composite film is 5% to 20%.

[0015] Preferably, the physical blending method includes mechanical stirring, magnetic stirring and ultrasonic dispersion.

[0016] Preferably, the hypercrosslinked polymer is one of a 4,4'-bis(chloromethyl)-1,1'-biphenyl hypercrosslinked polymer and a 1,4-bis(chloromethyl)phenyl hypercrosslinked polymer having a microporous structure. The hypercrosslinked polymer has a specific surface area of ​​800-1800 m 2 g -1 .

[0017] Preferably, the temperature of the amidation treatment is 60 to 300° C., and the amidation reaction time is 1 to 5 hours.

[0018] The present invention provides a low dielectric constant hypercrosslinked polymer / polyimide composite film for high frequency use prepared by the preparation method described in the above technical solution, and the composite film can be used in the fields of integrated circuits, microelectronics and insulating materials.

[0019] The present invention mixes diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and a non-protonic solvent, performs polymerization reaction by physical blending method, obtains a precursor polyamic acid solution, then adds a hyper-crosslinked polymer, and obtains a polyamic acid composite solution containing a hyper-crosslinked polymer by physical blending; the prepared polyamic acid composite solution is coated on a glass plate and subjected to step-wise heating to perform an amidation reaction, and the target composite film is obtained after peeling from the glass plate. The hyper-crosslinked polymer added in the present invention can introduce air into the composite film due to its high surface area and microporous structure, thereby reducing the dielectric constant of the composite film, while maintaining the mechanical properties and thermal stability of the composite film. The embodiment shows that the dielectric constant of the polyimide composite film prepared by the present invention is 1.6-2.5 in the range of 8.2-12.4GHz. At the same time, its T 5% The tensile strength and tensile modulus are 92 MPa and 2.15 GPa at 453 °C, respectively, indicating that the composite film maintains excellent thermodynamic and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Fourier transform infrared spectra of the films prepared in Examples 1 and 2 of the present invention and Comparative Example 1;

[0021] Figure 2 The curves showing the dielectric constants of the films prepared in Examples 2 and 3 of the present invention and Comparative Example 1 as a function of frequency;

[0022] Figure 3 The TGA curves of the films prepared in Examples 1 and 2 of the present invention and Comparative Example 1;

[0023] Figure 4 The tensile strength histogram of the films prepared in Example 1 of the present invention and Comparative Example 1;

[0024] Figure 5 The tensile modulus histogram of the films prepared in Example 2 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0025] The invention provides a method for preparing a low dielectric constant hypercrosslinked polymer / polyimide composite film under high frequency, comprising the following steps: mixing diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and a non-protonic solvent, performing a polymerization reaction by a physical blending method to obtain a precursor polyamic acid solution, then adding a hypercrosslinked polymer to the precursor solution, and performing physical blending to obtain a polyamic acid composite solution containing the hypercrosslinked polymer; scraping the prepared polyamic acid composite solution on a glass plate and stepwise heating the solution to perform an amidation reaction, and then peeling the solution from the glass plate and drying the solution to obtain a target composite film.

[0026] Unless otherwise specified, the present invention has no particular limitation on the sources of the components, and commercially available products known to those skilled in the art may be used.

[0027] In the present invention, the mass ratio of diaminodiphenyl ether to hexafluoroisopropylene diphthalic anhydride is 1:(2.3-2.5). The present invention limits the mass ratio of diaminodiphenyl ether to hexafluoroisopropylene diphthalic anhydride within the above range, which can make the diamine monomer and the dianhydride monomer fully react, adjust the structure of the polyimide, and improve the performance and stability of the polyimide composite film.

[0028] In the present invention, the hyper-crosslinked polymer has a high specific surface area and a microporous structure, and its specific surface area ranges from 800 to 1800 m 2 g -1 .

[0029] The present invention has no particular limitation on the source of the hyper-crosslinked polymer, as long as its surface area and pore size are close to or larger than the above ranges.

[0030] In the present invention, the mass content of the hyper-crosslinked polymer in the composite film is 5% to 20%, which can adjust the dispersion of the hyper-crosslinked polymer in the fluorinated polyimide matrix, further reduce the dielectric constant of the composite film, and at the same time make the composite film have excellent heat resistance and mechanical properties.

[0031] In the present invention, the hexafluoroisopropylene diphthalic anhydride is used as a dianhydride monomer, and diaminodiphenyl ether is used as a diamine monomer to react to generate polyimide. In the present invention, the hexafluoroisopropylene diphthalic anhydride contains a biphenyl structure, which can improve the thermal stability and mechanical properties of the composite film, and the trifluoromethyl group in the dianhydride monomer and the ether bond in the diamine monomer can reduce the polarizability, thereby reducing the dielectric constant.

[0032] In the present invention, the solvent preferably includes one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone, and more preferably N,N-dimethylacetamide.

[0033] In the present invention, when the diamine monomer, the dianhydride monomer and the aprotic solvent are physically blended, the ratio of diaminodiphenyl ether to the solvent is 1g:(9-10)mL. The present invention limits the mass concentration of diaminodiphenyl ether to the above range, which is conducive to the dispersion of the hyper-crosslinked polymer and to obtain a composite film with good performance after subsequent high-temperature amidation.

[0034] In the present invention, the polymerization reaction is carried out in two steps, wherein the temperature of the initial polymerization reaction is preferably -5 to 5°C, and the second step polymerization reaction is preferably room temperature (25°C). The polymerization reaction time is preferably 5 to 10 hours, more preferably 5 to 8 hours. The present invention limits the polymerization reaction temperature and time within the above range, which can make the reaction proceed more fully.

[0035] After the polymerization reaction is completed, the present invention preferably removes bubbles from the product of the polymerization reaction and then compounds it to obtain a polyamic acid composite solution.

[0036] In the present invention, the precursor polyamic acid solution needs to be degassed after the polymerization reaction, and the degassed process is performed by standing the solution at room temperature for 12 to 48 hours, preferably 24 hours.

[0037] In the present invention, the film-forming by scraping is preferably carried out on a dry and clean glass plate. In the present invention, the film-forming by scraping is carried out on a scraping machine.

[0038] After obtaining the polyamic acid composite solution, the present invention performs an amidation treatment on the polyamic acid composite solution to obtain a polyimide composite film.

[0039] In the present invention, the temperature of the amidation treatment is preferably 60-300°C, and the time of the amidation treatment is preferably 1-5 hours; more preferably, it is kept at 60°C for 40 minutes, 100°C for 1 hour, 200°C for 1 hour, and 300°C for 1 hour. In the present invention, the heating rate during the amidation treatment is preferably 5°C / min. The present invention limits the temperature, time and heating rate of the amidation treatment within the above range, so that the amidation reaction can be fully carried out to obtain a polyimide composite film with good film-forming properties.

[0040] The present invention has no special requirements for the equipment of the amidation treatment, and equipment familiar to those skilled in the art can be used. In the present invention, the amidation treatment is preferably carried out in a muffle furnace.

[0041] After the amidation treatment is completed, the present invention preferably sequentially cools, strips and dries the amidation product to obtain a polyimide composite film.

[0042] In the present invention, the cooling is preferably natural cooling, and the end point of the cooling is preferably room temperature.

[0043] In the present invention, the drying is preferably air-blast drying, the drying temperature is preferably 60° C., and the drying time is preferably 1 to 3 hours, more preferably 2 hours.

[0044] The present invention adds a hyper-crosslinked polymer during the reaction process (in the precursor), which can make the hyper-crosslinked polymer more evenly dispersed in the composite film, control the mass content of the hyper-crosslinked polymer, introduce air without causing agglomeration, thereby reducing the dielectric constant of the composite film, control the raw material composition and the process parameters of each step, and adjust the structure of the polyimide, so that the composite film has higher thermal stability and mechanical properties.

[0045] The present invention provides a low dielectric constant hypercrosslinked polymer / polyimide composite film for use at high frequencies prepared by the preparation method described in the above technical solution. In the present invention, the thickness of the polyimide composite film is preferably 15 to 25 μm.

[0046] The polyimide composite film prepared by the invention has lower dielectric constant and better thermal stability and mechanical properties.

[0047] The present invention also provides the application of the low dielectric constant hypercrosslinked polymer / polyimide composite film in the fields of integrated circuits, microelectronics and insulating materials described in the above technical solution. The present invention has no special limitation on the application of the low dielectric constant hypercrosslinked polymer / polyimide composite film in the fields of integrated circuits, microelectronics and insulating materials, and the technical solution of the application of polyimide composite film in the fields of integrated circuits, microelectronics and insulating materials well known to those skilled in the art can be adopted.

[0048] The technical solution of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] Dissolve 2.0g of 4,4'-diaminodiphenyl ether in 18mL of N,N-dimethylformamide and sonicate for 30 minutes until completely dissolved; then slowly add 4.6g of 4,4'-(hexafluoroisopropylene) diphthalic anhydride in a low-temperature constant temperature water bath at -5°C. Stir for about 1 hour, and when the pole climbing phenomenon appears, place the above mixed system in a room temperature environment and continue stirring for 5 hours to obtain a viscous polyamic acid solution. Let it stand at room temperature for 24 hours to remove bubbles. Take 2g of polyamic acid solution, add 0.03g of 4,4'-bis(chloromethyl)-1,1'-biphenyl super cross-linked polymer (specific surface area of ​​1800m 2 g -1 ), magnetic stirring for 30 minutes and then ultrasonic dispersion for 2 hours, so that the hyper-crosslinked polymer is more evenly dispersed in the polyamic acid solution, and a polyamic acid composite solution containing a hyper-crosslinked polymer is obtained. The polyamic acid composite solution is then cast on a dry and clean glass plate, and a film is formed by a scraping machine, with a film thickness of about 300 μm, and placed in a muffle furnace, and thermal amidation is performed within a temperature gradient of 60 to 300°C (60°C for 40 minutes, 100°C, 200°C, and 300°C for 1 hour each, and the heating rate is 5°C / min). After naturally cooling to room temperature, the film is peeled off, and then dried at 60°C for 2 hours to obtain a polyimide composite film in which the mass of the hyper-crosslinked polymer accounts for 5% of the composite film, which is recorded as a 5% HCP-FPI composite film, with a film thickness of 15 μm. In the entire X-band (8.2-12.4GHz), its dielectric constant is 2.2-2.8, T 5% The temperature is 483℃ and the tensile strength is 92MPa.

[0051] Example 2

[0052] Dissolve 2.0g of 4,4'-diaminodiphenyl ether in 18mL of N,N-dimethylacetamide and sonicate for 30min until completely dissolved; then slowly add 4.6g of 4,4'-(hexafluoroisopropylene) diphthalic anhydride in a 0℃ ice water bath and stir for about 1h. When the pole climbing phenomenon appears, place the above mixed system in a room temperature environment and continue stirring for 5h to obtain a viscous polyamic acid solution. Let it stand at room temperature for 24h to remove bubbles. Take 2g of polyamic acid solution, add 0.062g of 4,4'-bis(chloromethyl)-1,1'-biphenyl hypercrosslinked polymer (specific surface area of ​​1800m 2 g -1), magnetic stirring for 30 minutes and then ultrasonic dispersion for 2 hours, so that the hyper-crosslinked polymer is more evenly dispersed in the polyamic acid solution, and a polyamic acid composite solution containing a hyper-crosslinked polymer is obtained. The polyamic acid composite solution is then cast on a dry and clean glass plate, and a film is formed by scraping with a scraper, with a film thickness of about 300 μm, and placed in a muffle furnace, and thermal amidation is performed within a temperature gradient of 60 to 300°C (60°C for 40 minutes, 100°C, 200°C, and 300°C for 1 hour each, and a heating rate of 5°C / min). After naturally cooling to room temperature, the film is peeled off, and then dried at 60°C for 2 hours to obtain a polyimide composite film, which is recorded as a 10% HCP-FPI composite film with a film thickness of 20 μm. In the entire X-band (8.2-12.4GHz), its dielectric constant is 1.6-2.5, T 5% The temperature is 453℃ and the tensile modulus is 2.15GPa.

[0053] Example 3

[0054] Dissolve 2.0g of 4,4'-diaminodiphenyl ether in 19mL of N,N-dimethylacetamide and sonicate for 30min until completely dissolved; then slowly add 4.8g of 4,4'-(hexafluoroisopropylene) diphthalic anhydride in a 0℃ ice water bath and stir for about 1h. When the pole climbing phenomenon appears, place the above mixed system in a room temperature environment and continue stirring for 5h to obtain a viscous polyamic acid solution. Let it stand at room temperature for 24h to remove bubbles. Take 2g of the polyamic acid solution, add 0.099g of 1,4-bis(chloromethyl)phenyl super cross-linked polymer (specific surface area of ​​800m 2 g -1 ), magnetic stirring for 30 minutes and then ultrasonic dispersion for 2 hours, so that the hyper-crosslinked polymer is more evenly dispersed in the polyamic acid solution, and a polyamic acid composite solution containing a hyper-crosslinked polymer is obtained. The polyamic acid composite solution is then cast on a dry and clean glass plate, and a film is formed by a scraping machine, with a film thickness of about 300 μm, and placed in a muffle furnace, and thermal amidation is performed within a temperature gradient of 60 to 300°C (60°C for 40 minutes, 100°C, 200°C, and 300°C for 1 hour each, and the heating rate is 5°C / min). After naturally cooling to room temperature, the film is peeled off, and then dried at 60°C for 2 hours to obtain a polyimide composite film, which is recorded as a 15% HCP-FPI composite film with a film thickness of 20 μm. In the entire X-band (8.2-12.4GHz), its dielectric constant is 1.7-2.5, T 5% It is 444℃.

[0055] Example 4

[0056] Dissolve 2.0g of 4,4'-diaminodiphenyl ether in 20mL of N-methylpyrrolidone and sonicate for 30min until completely dissolved; then slowly add 5.0g of 4,4'-(hexafluoroisopropylene) diphthalic anhydride in a low-temperature constant temperature water bath at 5°C and stir for about 1h. When the climbing phenomenon appears, place the above mixed system in a room temperature environment and continue stirring for 5h to obtain a viscous polyamic acid solution. Let it stand at room temperature for 24h to remove bubbles. Take 2g of polyamic acid solution, add 0.140g of 4,4'-bis(chloromethyl)-1,1'-biphenyl super cross-linked polymer (specific surface area of ​​1800m 2 g -1 ), magnetic stirring for 30 minutes and then ultrasonic dispersion for 2 hours, so that the hyper-crosslinked polymer is more evenly dispersed in the polyamic acid solution, and a polyamic acid composite solution containing a hyper-crosslinked polymer is obtained. The polyamic acid composite solution is then cast on a dry and clean glass plate, and a film is formed by scraping with a scraper, with a film thickness of about 300 μm, and placed in a muffle furnace, and thermal amidation is performed within a temperature gradient of 60 to 300°C (60°C for 40 minutes, 100°C, 200°C, and 300°C for 1 hour each, and a heating rate of 5°C / min). After naturally cooling to room temperature, the film is peeled off, and then dried at 60°C for 2 hours to obtain a polyimide composite film, which is recorded as a 20% HCP-FPI composite film with a film thickness of 25 μm. Its dielectric constant is 2.2-3.0 in the entire X-band (8.2-12.4GHz), T 5% It is 425℃.

[0057] Comparative Example 1

[0058] In Comparative Example 1, no hyper-cross-linked polymer is added, and other parameters are the same as those in Example 1, to obtain a polyimide film, denoted as FPI film, with a film thickness of 20 μm and a dielectric constant of 2.3-3.0 at 8.2-12.4 GHz, indicating that the dielectric constant at high frequencies can be significantly reduced by uniformly compounding hyper-cross-linked polymers.

[0059] The Fourier transform infrared spectra of the films prepared in Examples 1 and 2 and Comparative Example 1 were tested. The prepared films were cut into small pieces of 30 mm × 30 mm and tested using a Fourier transform infrared spectrometer with a scanning range of 2000 to 500 cm -1 , the results are as follows Figure 1 As shown. Figure 1 It can be seen that the four IR absorption peaks are at 1783 cm -1 (asymmetric stretching vibration of the C=O double bond of the imide ring), 1716 cm -1 (symmetric stretching vibration of C=O double bond of imide ring), 1372 cm -1 (imide ring CN bond stretching vibration), 720cm -1(bending vibration within the imide ring plane), these four IR absorption peaks together constitute the characteristic peaks of PI. The polyimide film is successfully prepared by the preparation method of the present invention.

[0060] The dielectric properties of the films prepared in Examples 3 and 4 and Comparative Example 1 were measured by a vector network analyzer in the frequency range of 8.2 GHz to 12.4 GHz. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the dielectric constants of the composite films prepared by the present invention are relatively low. When the doping amount of the hyper-crosslinked polymer is 10wt%, the dielectric constant of the composite film can be reduced to 1.6-2.5 in the entire X-band (8.2-12.4GHz); the dielectric constant of the composite film can only be reduced when it is within the hyper-crosslinked polymer content range specified by the present invention.

[0061] The TGA curves of the films prepared in Examples 1 and 2 and Comparative Example 1 were tested. The thermogravimetric analysis (TGA) of the composite films was performed using TGA / DSC 2 in air at a heating rate of 10°C / min. The results are shown in FIG. Figure 3 The 5% thermal decomposition temperature (T 5% ) are relatively high. When the incorporation amount of the hypercrosslinked polymer is 10wt%, the T 5% can still be maintained at 453℃; with the increase of doping amount, the T 5% It dropped slightly, but still remained above 425℃.

[0062] The mechanical properties of the films prepared in Examples 1, 2 and Comparative Example 1 were measured using a universal testing machine at a strain rate of 2 mm / min. The length and width of the samples were 25 mm and 5 mm, respectively. The average value of five measurements was taken for each sample. The results are shown in Table 1. Figure 4 , 5 The composite film prepared by the present invention has good overall mechanical properties. When the incorporation amount of the hypercrosslinked polymer is 5wt%, the tensile strength of the composite film is 92MPa; when the incorporation amount of the hypercrosslinked polymer is 10wt%, the tensile modulus of the composite film is 2.15GPa; only when the content of the hypercrosslinked polymer is within the range defined by the present invention can the good mechanical properties be maintained.

[0063] In summary, the composite film prepared by the present invention has a lower dielectric constant and better thermal stability and mechanical properties at high frequencies.

[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a low dielectric constant hypercrosslinked polymer / polyimide composite film at high frequencies, characterized in that: The steps include: The diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and a non-protonic solvent are mixed by a physical mixing method to carry out a polymerization reaction to obtain a precursor polyamic acid solution; Adding a hyper-crosslinked polymer to a precursor polyamic acid solution and physically blending the mixture to obtain a polyamic acid composite solution containing the hyper-crosslinked polymer; The hypercrosslinked polymer is one of a 4,4'-bis(chloromethyl)-1,1'-biphenyl hypercrosslinked polymer and a 1,4-bis(chloromethyl)phenyl hypercrosslinked polymer having a microporous structure; the hypercrosslinked polymer has a specific surface area of ​​800-1800 m 2 g -1 ; The mass content of the hyper-crosslinked polymer in the composite film is 5% to 15%; The polyamic acid composite solution containing a hyper-crosslinked polymer is coated on a glass plate and the temperature is increased stepwise to undergo an amidation reaction, and then the solution is peeled off from the glass plate and dried to obtain a hyper-crosslinked polymer / polyimide composite film with a low dielectric constant at high frequencies.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the diaminodiphenyl ether to hexafluoroisopropylene diphthalic anhydride in step (1) is 1:(2.3-2.5).

3. The preparation method according to claim 1, characterized in that: The aprotic solvent in step (1) is one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

4. The preparation method according to claim 1, characterized in that: When the diaminodiphenyl ether, hexafluoroisopropylene diphthalic anhydride and the aprotic solvent are physically blended in step (1), the ratio of diaminodiphenyl ether to the solvent is 1 g: (9-10) mL.

5. The preparation method according to claim 1, characterized in that: The polymerization reaction of diaminodiphenyl ether and hexafluoroisopropylene diphthalic anhydride in step (1) is firstly carried out at a temperature of -5 to 5°C for 1 to 2 hours, and then at room temperature for 4 to 8 hours.

6. The preparation method according to claim 1, characterized in that: The physical blending method is one or more of mechanical stirring, magnetic stirring and ultrasonic dispersion.

7. The preparation method according to claim 1, characterized in that: The temperature of the amidation reaction in step (3) is 60-300° C., and the time of the amidation reaction is 1-5 h.

8. A polyimide composite film with low dielectric constant for high frequency prepared by the preparation method according to any one of claims 1 to 7, wherein the polyimide composite film with low dielectric constant for high frequency is used in the fields of integrated circuits, microelectronics and insulating materials.