Photovoltaic cell front silver paste and preparation method thereof, electrode and photovoltaic cell
By using spherical silver-clad copper powder and ultrasonic treatment technology, the fluidity of the conductive coating is improved, and the adhesion and conductivity of the photovoltaic cell electrode are enhanced through plasma treatment, solving the problem of network blocking caused by the high viscosity of the conductive coating. .
Patent Information
- Application Number
- CN202211150489.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-21
AI Technical Summary
The existing conductive coating has a high viscosity, which makes it easy to cause network blockage during screen printing. How to improve the fluidity of conductive paste has become a technical problem that needs to be solved urgently.
Spherical silver-clad copper powder is used to replace conventional special-shaped silver powder, and ultrasonic treatment is carried out during mixing and rolling to reduce the viscosity of the slurry and improve fluidity. At the same time, plasma treatment is performed on the front of the photovoltaic cell to enhance the silver paste and substrate. Adhesion and conductivity.
It effectively reduces the viscosity of silver paste, improves fluidity, reduces the probability of network blocking, and improves the binding force and conductivity of silver paste with substrate through ultrasonic treatment and plasma treatment.
Smart Images

Figure CN115512874B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of electronic pastes, and more specifically, relates to a photovoltaic cell front silver paste and a preparation method thereof, an electrode and a photovoltaic cell. Background Art
[0002] In recent years, the development of the electronics field in countries around the world has been rapid, among which the development of conductive paste has played a decisive role in the development of the electronics field in various countries. The most commonly used conductive pastes at home and abroad are mostly based on Ag as the conductive phase, and many conductive pastes are also prepared around Ag, but the cost of Ag is relatively high. In comparison, Cu has better conductivity and is cheap, but the conductivity of Cu oxide is far from that of Ag oxide. Therefore, using Ag to coat Cu to prepare the corresponding conductive paste can greatly reduce costs and effectively maintain conductivity.
[0003] Nowadays, economic development has become the main focus of all countries, but development at the expense of the environment and energy is also what countries do not want to see. At the same time, solar energy as a sustainable energy has entered people's field of vision. As a safe, clean, huge reserve and renewable energy, solar energy has huge development potential. Conductive coating, as a key part that determines the photoelectric conversion efficiency of crystalline silicon solar photovoltaic panels, plays a vital role in the entire photovoltaic field.
[0004] The conductive coating is generally printed on the surface of the battery cell by screen printing. In the prior art, the viscosity of the conductive coating is high and the corresponding fluidity is generally biased, which can easily cause screen clogging during the screen printing process. How to improve the fluidity of the conductive coating slurry has become a technical problem that urgently needs to be solved. Summary of the invention
[0005] The purpose of the embodiments of the present application is to provide a photovoltaic cell front silver paste and a preparation method thereof, aiming to solve the technical problem of poor fluidity of the silver paste.
[0006] To achieve the above-mentioned purpose, the technical solution adopted in this application is: to provide a photovoltaic cell front silver paste, which, calculated by weight, comprises: 3-8 parts of epoxy resin, 2-7 parts of additives and 85-95 parts of spherical silver-coated copper powder.
[0007] As a solution of some embodiments, the D90 particle size of the spherical silver-coated copper powder is 0.5-1 μm.
[0008] As a scheme of some embodiments, the epoxy resin includes one or a combination of at least two of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 1,2-epoxy-4-vinylcyclohexane and bisphenol A type epoxy resin.
[0009] As a solution of some embodiments, the auxiliary agent includes a solvent, a defoamer, a dispersant and a leveling agent in a mass ratio of (20-30): (1-3): (1-3): (2-3).
[0010] As a scheme of some embodiments, the solvent includes one or a combination of at least two of diethylene glycol diethyl ether, diethylene glycol butyl ether acetate, dimethyl adipate, diethylene glycol butyl ether, n-hexane and toluene.
[0011] As a solution of some embodiments, the defoaming agent includes one of BYK-022, BYK-024, BYK-141, or a combination of at least two thereof.
[0012] As a solution of some embodiments, the dispersant includes one of BYK-204, 5040, 5027, or a combination of at least two thereof.
[0013] As solutions of some embodiments, the leveling agent includes any one of J2102, BYK3560, BYK3700, or a combination of at least two of them.
[0014] Another object of the present application is to provide a method for preparing silver paste for the front side of a photovoltaic cell, and to further solve the problem of poor fluidity of the silver paste by improving the preparation method. The method for preparing silver paste for the front side of a photovoltaic cell comprises the following steps:
[0015] The epoxy resin, the additive and the spherical silver-coated copper powder are evenly mixed to obtain the front silver paste.
[0016] As a solution of some embodiments, ultrasonic treatment is performed synchronously during the mixing process.
[0017] The above-mentioned mixing method includes but is not limited to stirring mixing, the stirring speed is 100-2000rpm, and the stirring time is 10-60min.
[0018] The above-mentioned mixing method may also include rolling treatment, and the rolling process may be carried out using a three-roll rolling mill, and the rolling may be combined with stirring and mixing.
[0019] Another object of the present application is to provide an electrode to solve the problem of poor adhesion and poor conductivity between silver paste and materials.
[0020] Specifically, the electrode is obtained by sintering the above-mentioned photovoltaic cell front silver paste on the front side of the photovoltaic cell.
[0021] As a solution of some embodiments, the front side of the photovoltaic cell is subjected to plasma treatment before the photovoltaic cell front side paste is attached.
[0022] As a solution of some embodiments, the plasma treatment can be performed using inert gas plasma, where the inert gas includes one or a mixture of nitrogen, argon, helium, neon, krypton, and xenon. It can also be performed using oxygen plasma.
[0023] As a solution of some embodiments, the plasma treatment adopts oxygen plasma.
[0024] As a solution of some embodiments, the plasma treatment time is 1-10 minutes.
[0025] Another object of the application is to provide a photovoltaic cell having the above-mentioned electrode, wherein the photovoltaic cell includes the above-mentioned electrode.
[0026] In summary, the present application includes at least one of the following beneficial technical effects:
[0027] 1. The photovoltaic cell front silver paste of the present invention adopts spherical silver-coated copper powder to replace other special-shaped silver powders in conventional technology, which reduces the resistance between the material particles in the silver paste, thereby improving the fluidity of the paste and reducing the viscosity of the paste. The obtained paste is also more suitable for screen printing and can reduce the probability of screen blocking.
[0028] 2. On the other hand, in the preparation method of the photovoltaic cell front silver paste of the present invention, the viscosity of the slurry is effectively reduced by simultaneously performing ultrasonic treatment during the mixing and rolling processes. Analysis shows that this may be due to cavitation generated inside the slurry during the ultrasonic treatment. The bubbles generated by the cavitation will cause the long-chain molecules in the slurry to break during the rupture process, thereby reducing the viscosity. Secondly, ultrasonic treatment can help make the mixing more uniform. During the ultrasonic treatment, collisions between molecules can convert mechanical energy into thermal energy, and heat and temperature rise can also reduce the viscosity of the slurry.
[0029] 3. The present invention also provides an electrode and a photovoltaic cell having the electrode. Before forming the corresponding electrode, it also includes a step of plasma treating the front side of the cell, thereby making the bonding between the cell substrate and the silver paste tighter, and further reducing the resistance between the substrate and the silver paste. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 The present invention is a flow chart of the method for forming the front electrode of the photovoltaic cell. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0033] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.
[0034] In addition, the mass of the relevant components mentioned in the description of the embodiments of the present invention can not only refer to the specific content of each component, but also represent the proportional relationship between the masses of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the mass described in the description of the embodiments of the present invention can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0035] On the one hand, an embodiment of the present application provides a photovoltaic cell front silver paste, which includes 3-8 parts of epoxy resin, 2-7 parts of additives and 85-95 parts of spherical silver-coated copper powder, calculated by weight, wherein only spherical silver-coated copper powder is used instead of filamentary or flaky silver-coated copper powder, which can greatly improve the problem of poor fluidity, thereby reducing viscosity and avoiding the problem of screen clogging caused by the silver paste during screen printing.
[0036] In one embodiment, the D90 particle size of the spherical silver-coated copper powder is 0.5-1 μm, and in the exemplary embodiment, the mass ratio of silver to copper in the spherical silver-coated copper powder is 1: 1. The silver-coated copper powder of this size not only has good dispersibility, but also can maintain the stability of the slurry suspension system, the slurry can be smoothly and evenly extruded from the printing mesh, and the printing pattern can be kept stable after extrusion before drying, thereby maintaining a relatively stable aspect ratio of the printed pattern lines.
[0037] In one embodiment, the epoxy resin includes one or more of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 1,2-epoxy-4-vinylcyclohexane and bisphenol A epoxy resin. After the spherical silver-coated copper powder is used to replace the flaky silver-coated copper powder, the fluidity of the silver paste is improved when other components remain unchanged, but the adhesion and conductivity between the silver paste and the photovoltaic cell substrate are reduced. The epoxy resins used above all have strong reactive epoxy groups, and it is easier to form a stable chemical bond during the contact between the silver paste and the substrate, so that the contact between the silver paste and the substrate is improved and the adhesion is enhanced.
[0038] In one embodiment, the additive includes a solvent, a defoamer, a dispersant, and a leveling agent in a mass ratio of (20-30):(1-3):(1-3):(2-3).
[0039] In one embodiment, the solvent includes one or a combination of at least two of diethylene glycol diethyl ether, diethylene glycol butyl ether acetate, dimethyl adipate, diethylene glycol butyl ether, n-hexane and toluene. The above solvents have good solubility in epoxy resin and a relatively slow evaporation rate, so that the slurry can maintain the stability of the printed pattern before drying and sintering, and can maintain a more uniform evaporation process of the solvent during the drying process, thereby avoiding disconnection of the printed pattern during the drying process.
[0040] In one embodiment, the defoaming agent includes one of BYK-022, BYK-024, BYK-141, or a combination of at least two thereof.
[0041] In one embodiment, the dispersant includes one of BYK-204, 5040, 5027, or a combination of at least two thereof.
[0042] In one embodiment, the leveling agent includes any one of J2102, BYK3560, BYK3700, or a combination of at least two thereof.
[0043] On the other hand, the present application also provides a method for preparing a front silver paste for a photovoltaic cell, the method for preparing the silver paste for the cell comprising the following steps:
[0044] Epoxy resin, additives and spherical silver-coated copper powder are mixed evenly to obtain a positive silver paste, and ultrasonic treatment is performed simultaneously during the mixing process. During the mixing process, ultrasound can make the particles in the paste vibrate. The particles vibrate and produce a superposition effect under the action of transverse waves, longitudinal waves and surface waves. In the superposition process, the particles in the sparse phase are subjected to the pulling force, thereby generating holes. In the process of the generation and disappearance of a large number of bubbles generated by cavitation, the particles on the surface of the bubbles will be subjected to extremely high pressure. These effects will not only generate heat, but also cause the long-chain polymer compounds in the raw materials to break bonds. The increase in temperature and the breaking of long-chain compounds will reduce the viscosity of the paste. At the same time, the local high temperature and high pressure brought by cavitation will also cause the silver-coated copper powder and the organic compound to react, and the reaction product can also further react in the process of combining with the photovoltaic cell substrate in the later stage, thereby helping to improve the contact performance and electrical properties between the silver paste and the substrate.
[0045] In one embodiment, the mixing method includes one or a combination of dynamic mixing and static mixing. Specifically, the dynamic mixing method includes but is not limited to stirring mixing and rolling mixing. The static mixing method includes but is not limited to mixing in a static mixer.
[0046] The method of simultaneously performing ultrasonic treatment during dynamic mixing includes: transmitting ultrasonic vibrations generated by an ultrasonic generator to the surface of the silver paste through a medium, and the medium includes but is not limited to a mixing device body, a gas medium, a liquid medium, a solid medium or a combination of the above.
[0047] The method of simultaneously performing ultrasonic treatment during static mixing includes: transmitting ultrasonic vibrations generated by an ultrasonic generator to the surface of a static mixer through a medium, wherein the medium includes but is not limited to a gas medium, a liquid medium, a solid medium or a combination thereof.
[0048] In one embodiment, the rolling process specifically includes feeding the raw materials of the slurry into a three-roll hydraulic slurry rolling mill for rolling treatment, and obtaining the silver paste after the rolling treatment.
[0049] In a third aspect, an embodiment of the present application further provides an electrode for a photovoltaic cell, wherein the electrode is attached to the front side of the photovoltaic cell using the above-mentioned front silver paste and sintered.
[0050] Specifically, the method for forming an electrode includes the following steps:
[0051] S1. Plasma treatment is performed on the front side of the photovoltaic cell;
[0052] S2. Attach silver paste on the front side of the photovoltaic cell to the front side of the photovoltaic cell, and obtain the photovoltaic cell after drying and sintering.
[0053] In a specific embodiment, the drying method includes: heating the photovoltaic cell with the front silver paste attached to 40-60°C, and completing the drying after heat preservation for 1±0.5h. The sintering method includes: heating the photovoltaic cell with the front silver paste attached to 180±20°C, and completing the sintering after heat preservation for 3±0.5h.
[0054] In one embodiment, the method of attaching the electrode to the front side of the photovoltaic cell comprises a printing method, and as an example, a screen printing method is used, and as another example, a high-precision screen printing method is used.
[0055] In one embodiment, the front of the photovoltaic cell is also treated with plasma before the silver paste on the front of the photovoltaic cell is attached. The front substrate of the photovoltaic cell is generally made of crystalline silicon, and the silver paste needs to form an ohmic contact with the crystalline silicon in order to realize the electrode function after printing and sintering. The realization of ohmic contact in the prior art mainly lies in the close contact between the silver-coated copper particles and the crystalline silicon, which mainly depends on the binder (epoxy resin and additives) to provide sufficient adhesion, thereby reducing the distance between the silver-coated copper particles and the crystalline silicon. In order to reduce the viscosity, this embodiment uses spherical silver-coated copper powder, which makes the contact between the silver-coated copper powder and the crystalline silicon become point-to-surface contact, and the contact effect is extremely poor, thereby increasing the contact resistance. In order to overcome this problem, the surface of the photovoltaic cell is treated with plasma to form reaction sites on the surface of the device. After printing, the silver paste is not only simply contacted by adhesion, but the silver-coated copper powder can also react with the active sites on the surface of the crystalline silicon to form bonds, thereby improving the conductive performance. Furthermore, the ultrasonic treatment during the preparation of the silver paste forms reactive active points on the surface of the silver-coated copper powder in the silver paste, thereby also improving the contact performance between the silver-coated copper powder and the crystalline silicon.
[0056] In the above embodiments, plasma treatment can be carried out by inert gas plasma treatment, such as nitrogen plasma, argon plasma, etc., or oxygen plasma treatment can be carried out. Epoxy resin and solvent are both raw materials containing epoxy or oxygen groups, and oxygen plasma treatment forms oxygen-containing functional groups on the front of the photovoltaic cell. The introduction of these oxygen-containing functional groups makes the surface of the photovoltaic cell have better contact reaction performance with the epoxy resin and solvent in the silver paste. Compared with other plasma treatments, the surface of the photovoltaic cell treated with oxygen plasma is more reactive.
[0057] In one embodiment, the plasma treatment time is 1-10 minutes.
[0058] In a fourth aspect, the present invention further provides a photovoltaic cell having the electrode of the above embodiment, wherein the photovoltaic cell includes the electrode prepared by the above embodiment.
[0059] The technical solution of the present invention will be described below with specific embodiments:
[0060] Example 1
[0061] Preparation of additives: Weigh 25 parts of diethylene glycol butyl ether acetate, 1 part of BYK-022 defoamer, 1 part of BYK-204 dispersant, and 2 parts of J2102 leveling agent respectively, and mix them to obtain the additives.
[0062] Weigh 4 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4 parts of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 6 parts of additives, and 85 parts of spherical silver-coated copper powder (containing 50wt% silver) with a D90 particle size of 1μm respectively, add epoxy resin, additives and spherical silver-coated copper powder into a stirring tank for stirring, the stirring paddle speed is 600rpm, the stirring treatment is carried out for 30min, an ultrasonic generator is installed on the outer wall of the stirring tank, and the ultrasonic generator is turned on while stirring.
[0063] After stirring and mixing, the obtained mixture is added to the feed end of the three-roll hydraulic slurry mill. At the same time, an ultrasonic generator is connected to the roller end of the three-roll hydraulic slurry mill. The ultrasonic generator is turned on while rolling. After rolling is completed, the silver paste is obtained.
[0064] Example 2
[0065] Preparation of additives: Weigh 10 parts of diethylene glycol diethyl ether, 10 parts of dimethyl adipate, 2 parts of BYK-024 defoamer, 2 parts of 5040 dispersant, and 3 parts of BYK3560 leveling agent respectively, and mix them to obtain the additives.
[0066] 3 parts of 1,2-epoxy-4-vinylcyclohexane, 2 parts of an auxiliary agent, and 95 parts of spherical silver-coated copper powder (containing 50 wt% silver) with a D90 particle size of 0.5 μm were weighed respectively, and the epoxy resin, the auxiliary agent and the spherical silver-coated copper powder were added into a stirring tank for stirring. The stirring paddle speed was 100 rpm, and the stirring treatment was performed for 60 minutes. An ultrasonic generator was installed on the outer wall of the stirring tank, and the ultrasonic generator was turned on while stirring.
[0067] After stirring and mixing, the obtained mixture is added to the feed end of the three-roll hydraulic slurry mill. At the same time, an ultrasonic generator is connected to the roller end of the three-roll hydraulic slurry mill. The ultrasonic generator is turned on while rolling. After rolling is completed, the silver paste is obtained.
[0068] Example 3
[0069] Preparation of additives: Weigh 10 parts of diethylene glycol butyl ether, 10 parts of n-hexane, 10 parts of toluene, 2 parts of BYK-024 defoamer, 1 part of BYK-141 defoamer, 2 parts of 5040 dispersant, 1 part of 5027 dispersant, 1 part of BYK3560 leveling agent, and 2 parts of BYK3700 leveling agent respectively, and mix them to obtain the additives.
[0070] 8 parts of bisphenol A epoxy resin, 7 parts of auxiliary agent, and 90 parts of spherical silver-coated copper powder (containing 50 wt% silver) with a D90 particle size of 0.8 μm were weighed respectively, and the epoxy resin, auxiliary agent and spherical silver-coated copper powder were added to a stirring tank for stirring. The stirring paddle speed was 2000 rpm and the stirring treatment was performed for 10 minutes. An ultrasonic generator was installed on the outer wall of the stirring tank, and the ultrasonic generator was turned on while stirring.
[0071] After stirring and mixing, the obtained mixture is added to the feed end of the three-roll hydraulic slurry mill. At the same time, an ultrasonic generator is connected to the roller end of the three-roll hydraulic slurry mill. The ultrasonic generator is turned on while rolling. After rolling is completed, the silver paste is obtained.
[0072] Example 4
[0073] Preparation of additives: Weigh 25 parts of diethylene glycol butyl ether acetate, 1 part of BYK-022 defoamer, 1 part of BYK-204 dispersant, and 2 parts of J2102 leveling agent respectively, and mix them to obtain the additives.
[0074] Weigh 4 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4 parts of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 6 parts of additives, and 85 parts of spherical silver-coated copper powder (containing 50 wt% silver) with a D90 particle size of 1 μm respectively, add epoxy resin, additives and spherical silver-coated copper powder into a stirring kettle for stirring, the stirring paddle speed is 600 rpm, and the stirring treatment is carried out for 30 minutes.
[0075] After stirring and mixing, the obtained mixture is added to the feed end of a three-roll hydraulic slurry rolling mill, and rolling is completed to obtain a silver paste.
[0076] Example 5
[0077] Preparation of additives: Weigh 25 parts of diethylene glycol butyl ether acetate, 1 part of BYK-022 defoamer, 1 part of BYK-204 dispersant, and 2 parts of J2102 leveling agent respectively, and mix them to obtain the additives.
[0078] Weigh 4 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4 parts of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 6 parts of additives, and 85 parts of spherical silver-coated copper powder (containing 50wt% silver) with a D90 particle size of 1μm respectively, add epoxy resin, additives and spherical silver-coated copper powder into a stirring tank for stirring, the stirring paddle speed is 600rpm, the stirring treatment is carried out for 30min, an ultrasonic generator is installed on the outer wall of the stirring tank, and the ultrasonic generator is turned on while stirring.
[0079] After stirring and mixing, the obtained mixture is added to the feed end of a three-roll hydraulic slurry rolling mill, and rolling is completed to obtain a silver paste.
[0080] Example 6
[0081] Preparation of additives: Weigh 25 parts of diethylene glycol butyl ether acetate, 1 part of BYK-022 defoamer, 1 part of BYK-204 dispersant, and 2 parts of J2102 leveling agent respectively, and mix them to obtain the additives.
[0082] Weigh 4 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4 parts of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 6 parts of additives, and 85 parts of spherical silver-coated copper powder (containing 50 wt% silver) with a D90 particle size of 1 μm respectively, add epoxy resin, additives and spherical silver-coated copper powder into a stirring kettle for stirring, the stirring paddle speed is 600 rpm, and the stirring treatment is carried out for 30 minutes.
[0083] After stirring and mixing, the obtained mixture is added to the feed end of the three-roll hydraulic slurry mill. At the same time, an ultrasonic generator is connected to the roller end of the three-roll hydraulic slurry mill. The ultrasonic generator is turned on while rolling. After rolling is completed, the silver paste is obtained.
[0084] Comparative Example 1
[0085] Weigh 38 parts of an alkoxy-containing soluble phenolic resin (the number of carbon atoms of the alkoxy group is 4, the alkoxylation rate is 65%, and the weight-average molecular weight is 1200), 57 parts of a bisphenol F epoxy resin (epoxy equivalent is 170 g / eq), and 5 parts of 2-phenyl-4-methylimidazole, respectively, and mix them evenly to obtain an adhesive.
[0086] To 50 parts of the above adhesive, add 436.5 parts of silver-coated copper powder (containing 50 wt% silver), 13.5 parts of flat silver-coated copper powder (containing 50 wt% silver) and 15 parts of ethyl carbitol, and mix and disperse them evenly with a stirring stone mill and a three-roll mill to obtain a silver paste.
[0087] Comparative Example 2
[0088] Weigh 38 parts of an alkoxy-containing soluble phenolic resin (the number of carbon atoms of the alkoxy group is 4, the alkoxylation rate is 65%, and the weight-average molecular weight is 1200), 57 parts of a bisphenol F epoxy resin (the epoxy equivalent is 170 g / eq), and 5 parts of 2-phenyl-4-methylimidazole, respectively, and mix them evenly to obtain an adhesive. During the mixing process, an ultrasonic generator is used to apply ultrasonic treatment to the mixing cavity.
[0089] To 50 parts of the above adhesive, add 436.5 parts of silver-coated copper powder (containing 50 wt% silver), 13.5 parts of flat silver-coated copper powder (containing 50 wt% silver) and 15 parts of ethyl carbitol, and mix and disperse them evenly with a stirring stone mill and a three-roll mill to obtain a silver paste. During the stirring and dispersing process, ultrasonic treatment is applied.
[0090] The viscosity of the silver paste prepared above was tested and the following data were obtained:
[0091]
[0092] It can be seen from the data of the above embodiments that the silver paste of the present invention has a lower viscosity than the prior art (Comparative Example 1). At the same time, ultrasonic treatment is used in the preparation method of the silver paste of the present invention. Ultrasonic treatment can effectively reduce the viscosity of the silver paste. The main reasons may be cavitation, mechanical action and thermal action. Cavitation, that is, during the ultrasonic process, will cause negative pressure in certain areas of the slurry to form small bubbles. In the process from the formation to the rupture and disappearance of small bubbles, the change in the surface tension of the small bubbles will induce bond breaking of certain polymer compounds, thereby reducing the viscosity; at the same time, during the ultrasonic process, atoms will collide, and under the action of the collision, polymer bond breaking will also occur; and the thermal effect is due to the conversion of molecular collision kinetic energy into heat energy. Therefore, during the ultrasonic process, the temperature of the slurry will increase, thereby also being able to reduce the viscosity of the slurry.
[0093] Example 7
[0094] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 5 minutes, and then the silver paste prepared in Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0095] Example 8
[0096] The cell to be printed with silver paste was subjected to surface argon plasma treatment for 5 minutes, and then the silver paste prepared in Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0097] Example 9
[0098] The surface of the cell to be printed with silver paste was treated with nitrogen plasma for 5 minutes, and then the silver paste prepared in Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0099] Example 10
[0100] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 1 min, and then the silver paste prepared in Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60° C. for 1 h, and then sintered at 180° C. for 3 h to obtain a photovoltaic cell printed with silver paste.
[0101] Embodiment 11
[0102] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 10 minutes, and then the silver paste prepared in Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60° C. for 1 hour, and then sintered at 180° C. for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0103] Example 12
[0104] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 5 minutes, and then the silver paste prepared in Example 2 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0105] Embodiment 13
[0106] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 5 minutes, and then the silver paste prepared in Example 3 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0107] Embodiment 14
[0108] The silver paste prepared in Example 1 was printed onto the front of the cell by high-precision screen printing, dried in an oven at 40-60° C. for 1 h, and then sintered at 180° C. for 3 h to obtain a photovoltaic cell printed with silver paste.
[0109] Embodiment 15
[0110] The cell to be printed with silver paste was subjected to surface oxygen plasma treatment for 5 minutes, and then the silver paste prepared in Example 4 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0111] Example 16
[0112] The surface of the cell to be printed with silver paste was treated with oxygen plasma for 5 minutes, and then the silver paste prepared in Comparative Example 1 was printed on the front of the cell by high-precision screen printing, dried in an oven at 40-60°C for 1 hour, and then sintered at 180°C for 3 hours to obtain a photovoltaic cell printed with silver paste.
[0113] Comparative Example 3
[0114] The silver paste prepared in Comparative Example 1 was printed onto the front of the cell by high-precision screen printing, dried in an oven at 40-60° C. for 1 h, and then sintered at 180° C. for 3 h to obtain a photovoltaic cell printed with silver paste.
[0115] The photovoltaic cells prepared in the above-mentioned Examples 7-16 and Comparative Example 3 were respectively subjected to the silver paste adhesion test, and the adhesion test was carried out using the hundred-grid test method. At the same time, the corresponding electrodes were subjected to the volume resistivity test. The test results are shown in the following table:
[0116]
[0117] According to the test data of the battery cells prepared according to the above embodiments and comparative examples, it can be seen that the slurry after plasma treatment shows better contact performance. The reason for this may be that, on the one hand, the plasma will clean the surface of the substrate and remove the impurities on the surface, so that the substrate and the slurry can be more closely combined. Compared with nitrogen and argon plasma, the substrate treated with oxygen plasma shows better performance in reducing resistance. The reason may be that the oxygen plasma interacts with the surface of the substrate and is more likely to break the original chemical bonds of the substrate, thereby making it easier to introduce new functional groups on the surface of the substrate, which improves the bonding between the slurry and the substrate on the one hand, and reduces the contact resistance on the other hand. Secondly, according to the data comparison results of Example 7 and Comparative Example 2, it can be seen that the ultrasonic treatment in the preparation process of the silver paste will also affect the electrical properties between the silver paste and the substrate after printing. The experimental data of Example 14 and Example 15 show that under the same method of using the silver paste, the silver paste of the present invention and the silver paste of the prior art will still produce different adhesion and resistance. The experimental data of Example 15 and Example 16 show that although the silver paste of the prior art is used, the electrode obtained by the method of using the present invention still has better resistance and adhesion data.
[0118] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. An electrode, characterized in that: The electrode is obtained by sintering the front silver paste of the photovoltaic cell on the front of the photovoltaic cell; the front of the photovoltaic cell is treated with oxygen plasma before the front silver paste of the photovoltaic cell is attached; The photovoltaic cell front silver paste comprises, by weight, 3-8 parts of epoxy resin, 2-7 parts of auxiliary agent and 85-95 parts of spherical silver-coated copper powder. The preparation method of the photovoltaic cell front silver paste comprises the following steps: uniformly mixing the epoxy resin, auxiliary agent and spherical silver-coated copper powder to obtain the front silver paste; performing ultrasonic treatment simultaneously during the mixing process of the epoxy resin, auxiliary agent and spherical silver-coated copper powder; the auxiliary agent comprises a solvent, a defoamer, a dispersant and a leveling agent in a mass ratio of (20-30): (1-3): (1-3): (2-3); the solvent comprises one or a combination of at least two of diethylene glycol diethyl ether, diethylene glycol butyl ether acetate, dimethyl adipate, diethylene glycol butyl ether, n-hexane and toluene.
2. The electrode according to claim 1, characterized in that: The epoxy resin includes one or a combination of at least two of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 1,2-epoxy-4-vinylcyclohexane and bisphenol A type epoxy resin; and / or The D90 particle size of the spherical silver-coated copper powder is 0.5-1 μm.
3. The electrode according to claim 1 or 2, characterized in that: The defoamer comprises one of BYK-022, BYK-024, BYK-141 or a combination of at least two thereof; and / or The dispersant comprises one or a combination of at least two of BYK-204, 5040, and 5027; and / or The leveling agent includes any one of J2102, BYK3560, BYK3700 or a combination of at least two thereof.
4. A photovoltaic cell, characterized in that: Comprising the electrode as claimed in any one of claims 1 to 3.
Citation Information
Patent Citations
Coating for electromagnetic shielding, and preparation method and use method thereof
CN110951369A
Electrically conductive paste
CN111448670A
Conductive material, preparation method thereof and electronic device
CN112349447A
Method of manufacturing solar cell
JP2011192799A
Damp-heat-resistant and highly reliable conductive silver epoxy adhesive, method for preparing same, and application thereof
WO2017080040A1