High-order electrostatic dissipative carbon-based multi-component composite film material and preparation method thereof

The high-order static dissipative carbon-based multi-element composite thin film material prepared through anode layer ion source and non-equilibrium magnetron sputtering technology solves the problem of film peeling of semiconductor materials after heating, and achieves stable antistatic function and high nano-hardness. It meets the requirements of the semiconductor industry for electrostatic impedance and reduces production costs.

CN115522162BActive Publication Date: 2024-10-29SUZHOU HUIZHUAN NANO NEW MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211180581.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-26
Publication Date
2024-10-29
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

Existing semiconductor materials are prone to film peeling after heating and alkali cleaning, and the antistatic function cannot be continuously guaranteed. Moreover, the electrostatic impedance does not meet industry requirements, resulting in equipment damage and increased production costs.

Method used

Using two mixed vapor deposition technologies, anode layer ion source and non-equilibrium magnetron sputtering, a multi-component composite thin film material containing carbon, silicon, oxygen and titanium is prepared. The proportion and structure of the element components are adjusted to form a high-order electrostatic dissipative carbon-based multi-component. Composite film material with low friction coefficient, nano-hardness and stable antistatic resistance value.

Benefits of technology

It achieves the maintenance of film layer stability and antistatic function in the low to high temperature range, increases the nano-hardness, reduces the friction coefficient, complies with the electrostatic protection requirements of JEDEC standards, extends the service life of the material and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115522162B_ABST
    Figure CN115522162B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-order electrostatic dissipative carbon-based multi-component composite thin film material for the semiconductor field and a preparation method thereof, which solves the comprehensive technical difficulties of traditional thin film materials such as anodized layers and Teflon spray layers, such as excessively high resistance, poor surface wear resistance, and unstable chemical and temperature resistance. This material uses two different mixed gas deposition technologies, advanced anode layer ion source and unbalanced magnetron sputtering, and by adding silicon, oxygen, and titanium elements to the existing amorphous carbon-based thin film material, special process parameters are developed to prepare a special multi-component composite material with improved composition and structure, thereby meeting the comprehensive material performance requirements customized by customers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention specifically relates to a high-order electrostatic dissipative carbon-based multi-component composite thin film material for the semiconductor field and a preparation method thereof. Background Art

[0002] As the size of semiconductor components below 10 nanometers is miniaturized, their tolerance to static electricity is decreasing. The existing materials currently used in the industry, such as anodized layers and Teflon coatings, have too high surface resistance values. For example, local static electricity is easily accumulated on the surface of the carrier or carrier. These accumulated static charges cannot be conducted away in time, which will lead to abnormal discharge scenes, thereby directly damaging expensive chips and microcircuits. Once they are broken down, they cannot be repaired and can only be scrapped. Reprocessing a new chip or microcircuit requires very high production costs and a long production cycle, which greatly increases production and processing costs and reduces chip output. The new industry requires that the electrostatic impedance cannot be too high or too low, which is something that traditional materials cannot meet.

[0003] The semiconductor industry has very high cleanliness requirements for production equipment during the production and processing process. Some equipment components such as fixtures, carriers, carriers, guide rails, etc. are cleaned regularly. After heating and alkaline washing, the anodized layer and Teflon spray coating will peel off and can no longer guarantee the anti-static function. Therefore, the second pain point arises, requiring a new material with good chemical stability and thermal stability.

[0004] In addition, during long-term continuous production processes, inspection jigs or equipment components will wear out. Increasing their wear resistance can reduce the frequency of replacement and improve production efficiency. Summary of the invention

[0005] The purpose of the present invention is to address the shortcomings of existing materials and provide a high-order electrostatic dissipative carbon-based multi-component composite thin film material and a preparation method thereof, thereby solving the problem that after the existing semiconductor is heated and alkaline washed, the anodized layer and the Teflon spray layer will peel off and the antistatic function can no longer be guaranteed.

[0006] The present invention is achieved by: a high-order electrostatic dissipative carbon-based multi-component composite thin film material, wherein the high-order electrostatic dissipative carbon-based multi-component composite thin film material is prepared by using two different mixed gas phase deposition technologies, namely, an anode layer ion source and an unbalanced magnetron sputtering;

[0007] Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements;

[0008] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 72-78% carbon element, 12-18% silicon element, 5-10% oxygen element, and 0.5-3.5% titanium element.

[0009] Preferably, the high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 74-76% carbon element, 14-16% silicon element, 6-8% oxygen element, and 0.8-3% titanium element.

[0010] Preferably, the high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 75% carbon element, 15% silicon element, 7% oxygen element, and 2% titanium element.

[0011] Preferably, the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements, silicon, oxygen and titanium, and is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti), and has a variety of composite structures.

[0012] Preferably, the high-order electrostatic dissipative carbon-based multi-component composite film material structure comprises:

[0013] sp2 graphite phase structure;

[0014] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0015] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0016] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0017] Preferably, the nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1600HV-2000HV, the friction coefficient is 0.05-0.15, and the anti-static resistance value of the film layer is 10 5 -10 9 ohms, surface roughness is Ra0.1-0.2.

[0018] On the other hand, the present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0019] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0020] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0021] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0022] Preferably, the method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0023] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0024] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0025] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0026] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0027] Preferably, in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0028] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 50-150sccm, set the sputtering power of the titanium target to 5-20kW, load the bias voltage to 500-1200V, the pulse frequency to 10-150kHz and the duty cycle to 5-50%, and continue titanium plating for 10 minutes;

[0029] Step S202, continue sputtering titanium, adjust the argon flow rate to 50-150 sccm, the target power to 5-20 kW, and introduce acetylene at a flow rate of 100-350 sccm, and the transition layer lasts for 30 minutes;

[0030] Step S203, keep the magnetron sputtering titanium working, adjust the power to 5-20kW, turn on the anode layer ion source, set the voltage to 500-1500V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 2-10g / min, load bias to 500-1200V, pulse frequency 10-150kHz and duty cycle 5-50%, and deposition minutes is 250 minutes.

[0031] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0032] The material provided by the present invention adopts two different mixed vapor deposition technologies, namely, advanced anode layer ion source and unbalanced magnetron sputtering. By adding silicon, oxygen and titanium elements to the existing amorphous carbon-based thin film materials, special process parameters are developed to prepare special multi-component composite materials with improved composition and structure, thereby meeting the comprehensive material performance requirements customized by customers.

[0033] The antistatic resistance value of the high-order electrostatic dissipative carbon-based multi-component composite film material prepared in this application is precisely controlled within 10 5 -10 9 ohms range, in line with the industry testing standards of JEDEC-JESD625B, and the film will not peel off at low temperatures of -50°C to high temperatures of 200°C, and the resistance value can remain stable.

[0034] At the same time, the nanohardness of the high-order electrostatic dissipative carbon-based multi-composite film material prepared in this application reaches 1600HV-2000HV, and the friction coefficient is 0.05-0.15. These two performance indicators are far superior to traditional coating materials, thereby enhancing wear resistance and extending service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic structural diagram of the ESD-DLC carbon-based thin film material is shown.

[0036] Figure 2 A schematic structural diagram of a quaternary carbon-based thin film composite material containing carbon, hydrogen, silicon and oxygen is shown.

[0037] Figure 3 A surface energy comparison diagram of aC:H and aC:H:Si:O materials is shown.

[0038] Figure 4 A schematic diagram of the structure of a five-component carbon-based thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium is shown.

[0039] Figure 5 The graph shows the relationship between the surface resistance of the film and the titanium atom content.

[0040] Figure 6Shows the product nanohardness measurement curve.

[0041] Figure 7 The thickness measurement results of the film layer of this application are shown.

[0042] Figure 8 A standard diagram for judging film bonding strength is shown.

[0043] Fig. 9 A diagram showing the binding force of this product is shown. DETAILED DESCRIPTION

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0045] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0046] The purpose of the present invention is to address the shortcomings of existing materials and provide a high-order electrostatic dissipative carbon-based multi-component composite thin film material and a preparation method thereof, thereby solving the problem that after the existing semiconductor is heated and alkaline washed, the anodized layer and the Teflon spray layer will peel off and the antistatic function can no longer be guaranteed.

[0047] The high-order electrostatic dissipative carbon-based multi-component composite thin film material prepared in this application is specifically an electrostatic dissipative diamond-like carbon-based thin film material, which adopts two different mixed vapor deposition technologies of advanced anode layer ion source and unbalanced magnetron sputtering. The anode layer ion source technology can be used to prepare ultra-wear-resistant diamond-like carbon-based thin film materials with high hardness, low friction coefficient and very fine surface. This technology is more suitable for the vapor deposition of a variety of special mixed gases; and the technical feature of unbalanced magnetron sputtering is that by adjusting the power of magnetron sputtering, the ratio of specific element components can be more accurately modulated, and it is more suitable for the addition of alloy elements. Combining these two vapor deposition processes together can maximize their respective technical advantages and can more perfectly prepare new multi-component composite materials, such as Figure 1 As shown, a schematic structural diagram of the ESD-DLC carbon-based thin film material is shown.

[0048] Example 1

[0049] The embodiment of the present invention provides a high-order electrostatic dissipative carbon-based multi-component composite thin film material, which is prepared by using two different mixed vapor deposition technologies, namely, an anode layer ion source and an unbalanced magnetron sputtering. Combining these two vapor deposition processes together can maximize their respective technical advantages and more perfectly prepare a new multi-component composite material.

[0050] Among them, the anode layer ion source technology is used to prepare ultra-wear-resistant diamond-like carbon-based thin film materials with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of magnetron sputtering to ensure the modulation of a specific amount of element composition ratio, thereby facilitating the addition of alloy elements.

[0051] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 72% carbon element, 12% silicon element, 5% oxygen element, and 0.5% titanium element.

[0052] It should be noted that the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements, silicon, oxygen and titanium. It is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti), and has a variety of composite structures. These multiple composite structures meet the requirements of comprehensive performance.

[0053] Specifically, the high-order electrostatic dissipative carbon-based multi-component composite film material structure includes:

[0054] sp2 graphite phase structure;

[0055] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0056] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0057] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0058] The nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1600 HVHV, the friction coefficient is 0.05, and the anti-static resistance value of the film layer is 10 5 ohms, surface roughness is Ra0.1.

[0059] The present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0060] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0061] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0062] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0063] The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0064] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0065] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0066] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0067] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0068] It should be noted that in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0069] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 50 sccm, set the sputtering power of the titanium target to 5 kW, load the bias voltage to 500 V, the pulse frequency to 10 kHz and the duty cycle to 5%, and continue titanium plating for 10 minutes;

[0070] Step S202, continue sputtering titanium, adjust the argon flow rate to 50 sccm, the target power to 5 kW, and introduce acetylene at a flow rate of 100 sccm. The transition layer lasts for 30 minutes;

[0071] Step S203, keep the magnetron sputtering titanium working, adjust the power to 11kW, turn on the anode layer ion source, set the voltage to 500V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 2-10g / min, load bias to 500V, pulse frequency 10kHz and duty cycle 5%, deposition minutes is 250 minutes.

[0072] It should be noted that, in this embodiment, the raw materials for preparing the multi-component composite thin film material include solid sintered titanium target material, hexamethyldisiloxane, and amorphous diamond-like carbon-based thin film material, wherein the purity of titanium atoms in the solid sintered titanium target material is greater than 99.95%.

[0073] Example 2

[0074] The embodiment of the present invention provides a high-order electrostatic dissipative carbon-based multi-component composite thin film material, which is prepared by using two different mixed vapor deposition technologies: an anode layer ion source and unbalanced magnetron sputtering.

[0075] Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements;

[0076] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 78% carbon element, 18% silicon element, 10% oxygen element, and 3.5% titanium element.

[0077] It should be noted that the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements: silicon, oxygen and titanium. It is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti) and has a variety of composite structures.

[0078] The structure of high-order electrostatic dissipative carbon-based multi-component composite film materials includes:

[0079] sp2 graphite phase structure;

[0080] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0081] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0082] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0083] The nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 2000HV, the friction coefficient is 0.05-0.15, and the anti-static resistance value of the film layer is 10 9 ohms, surface roughness is Ra0.2.

[0084] The present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0085] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0086] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0087] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0088] The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0089] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0090] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0091] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0092] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0093] It should be noted that in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0094] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 150sccm, set the sputtering power of the titanium target to 20kW, load the bias voltage to 1200V, the pulse frequency to 150kHz and the duty cycle to 50%, and continue titanium plating for 10 minutes;

[0095] Step S202, continue sputtering titanium, adjust the argon flow rate to 150 sccm, the target power to 20 kW, and introduce acetylene at a flow rate of 350 sccm. The transition layer lasts for 30 minutes;

[0096] Step S203, keep the magnetron sputtering titanium working, adjust the power to 17kW, turn on the anode layer ion source, set the voltage at 1500V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 2-10g / min, load bias to 1200V, pulse frequency 150kHz and duty cycle 50%, deposition minutes is 250 minutes.

[0097] It should be noted that, in this embodiment, the raw materials for preparing the multi-component composite thin film material include solid sintered titanium target material, hexamethyldisiloxane, and amorphous diamond-like carbon-based thin film material, wherein the purity of titanium atoms in the solid sintered titanium target material is greater than 99.95%.

[0098] Example 3

[0099] The embodiment of the present invention provides a high-order electrostatic dissipative carbon-based multi-component composite thin film material, which is prepared by using two different mixed vapor deposition technologies: an anode layer ion source and unbalanced magnetron sputtering.

[0100] Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements;

[0101] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 74% carbon element, 14% silicon element, 6% oxygen element, and 0.8% titanium element.

[0102] It should be noted that the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements: silicon, oxygen and titanium. It is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti) and has a variety of composite structures.

[0103] The structure of high-order electrostatic dissipative carbon-based multi-component composite film materials includes:

[0104] sp2 graphite phase structure;

[0105] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0106] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0107] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0108] The nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1600HV-2000HV, the friction coefficient is 0.05, and the anti-static resistance value of the film layer is 10 5 ohms, surface roughness is Ra0.17.

[0109] The present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0110] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0111] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0112] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0113] The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0114] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0115] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0116] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0117] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0118] It should be noted that in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0119] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 50 sccm, set the sputtering power of the titanium target to 7 kW, load the bias voltage to 600 V, the pulse frequency to 18 kHz and the duty cycle to 20%, and continue titanium plating for 10 minutes;

[0120] Step S202, continue sputtering titanium, adjust the argon flow rate to 110 sccm, the target power to 17 kW, and introduce acetylene at a flow rate of 250 sccm. The transition layer lasts for 30 minutes;

[0121] Step S203, keep the magnetron sputtering titanium working, adjust the power to 12kW, turn on the anode layer ion source, set the voltage at 1400V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 9g / min, load bias to 900V, pulse frequency 130kHz and duty cycle 12%, and deposition minutes are 250 minutes.

[0122] It should be noted that, in this embodiment, the raw materials for preparing the multi-component composite thin film material include solid sintered titanium target material, hexamethyldisiloxane, and amorphous diamond-like carbon-based thin film material, wherein the purity of titanium atoms in the solid sintered titanium target material is greater than 99.95%.

[0123] Example 4

[0124] The embodiment of the present invention provides a high-order electrostatic dissipative carbon-based multi-component composite thin film material, which is prepared by using two different mixed vapor deposition technologies: an anode layer ion source and unbalanced magnetron sputtering.

[0125] Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements;

[0126] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 76% carbon element, 16% silicon element, 8% oxygen element, and 3% titanium element.

[0127] It should be noted that the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements: silicon, oxygen and titanium. It is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti) and has a variety of composite structures.

[0128] The structure of high-order electrostatic dissipative carbon-based multi-component composite film materials includes:

[0129] sp2 graphite phase structure;

[0130] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0131] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0132] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0133] The nano hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1600HV-2000HV, the friction coefficient is 0.09, and the anti-static resistance value of the film layer is 10 8 ohms, surface roughness is Ra0.17.

[0134] The present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0135] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0136] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0137] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0138] The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0139] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0140] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0141] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0142] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0143] It should be noted that in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0144] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 80 sccm, set the sputtering power of the titanium target to 16 kW, load the bias voltage to 650 V, the pulse frequency to 100 kHz and the duty cycle to 30%, and continue titanium plating for 10 minutes;

[0145] Step S202, continue sputtering titanium, adjust the argon flow rate to 110 sccm, the target power to 16 kW, and introduce acetylene at a flow rate of 220 sccm. The transition layer lasts for 30 minutes;

[0146] Step S203, keep the magnetron sputtering titanium working, adjust the power to 20kW, turn on the anode layer ion source, set the voltage at 1400V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 6g / min, load bias to 1050V, pulse frequency 17kHz and duty cycle 25%, deposition minutes is 250 minutes.

[0147] It should be noted that, in this embodiment, the raw materials for preparing the multi-component composite thin film material include solid sintered titanium target material, hexamethyldisiloxane, and amorphous diamond-like carbon-based thin film material, wherein the purity of titanium atoms in the solid sintered titanium target material is greater than 99.95%.

[0148] Example 5

[0149] The embodiment of the present invention provides a high-order electrostatic dissipative carbon-based multi-component composite thin film material, which is prepared by using two different mixed vapor deposition technologies: an anode layer ion source and unbalanced magnetron sputtering.

[0150] Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements;

[0151] The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 75% carbon element, 15% silicon element, 7% oxygen element, and 2% titanium element.

[0152] It should be noted that the high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements: silicon, oxygen and titanium. It is a high-order multi-component thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium (aC:H:Si:O:Ti) and has a variety of composite structures.

[0153] The structure of high-order electrostatic dissipative carbon-based multi-component composite film materials includes:

[0154] sp2 graphite phase structure;

[0155] sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials;

[0156] The second amorphous silicon-oxygen (a-Si:O) structure is formed after doping with silicon and oxygen;

[0157] The third amorphous titanium chain (a-Ti) structure formed by adding titanium element.

[0158] The nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1800 HV, the friction coefficient is 0.14, and the anti-static resistance value of the film layer is 10 7 ohms, surface roughness is Ra0.1.

[0159] The present application also provides a method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material, the method for preparing a high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprising:

[0160] Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials;

[0161] Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and an unbalanced magnetron sputtering technology;

[0162] Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120°C and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function.

[0163] The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes:

[0164] Step S101, taking raw materials for preparing multi-component composite thin film materials;

[0165] Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm;

[0166] Step S103, turning on two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the temperature control value of the thermocouple is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates;

[0167] Step S104, introduce argon gas, set the flow rate of argon gas to 250sccm, turn on the two rows of anode layer ion sources, set their voltage to 1200V, load a bias voltage of 800V, a pulse frequency of 40kHz and a duty cycle of 20% on the workpiece, and perform a 60-minute ion etching and cleaning process.

[0168] It should be noted that in the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes:

[0169] Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 150sccm, set the sputtering power of the titanium target to 20kW, load the bias voltage to 1200V, the pulse frequency to 150kHz and the duty cycle to 5%, and continue titanium plating for 10 minutes;

[0170] Step S202, continue sputtering titanium, adjust the argon flow rate to 50 sccm, the target power to 5 kW, and introduce acetylene at a flow rate of 100 sccm. The transition layer lasts for 30 minutes;

[0171] Step S203, keep the magnetron sputtering titanium working, adjust the power to 20kW, turn on the anode layer ion source, set the voltage at 1500V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 10g / min, load bias to 1200V, pulse frequency 10kHz and duty cycle 5%, deposition minutes is 250 minutes.

[0172] It should be noted that, in this embodiment, the raw materials for preparing the multi-component composite thin film material include solid sintered titanium target material, hexamethyldisiloxane, and amorphous diamond-like carbon-based thin film material, wherein the purity of titanium atoms in the solid sintered titanium target material is greater than 99.95%.

[0173] The antistatic resistance value of the high-order electrostatic dissipative carbon-based multi-component composite film material prepared in this application is precisely controlled within 10 5 -10 9 ohms range, in line with the industry testing standards of JEDEC-JESD625B, and the film will not peel off at low temperatures of -50°C to high temperatures of 200°C, and the resistance value can remain stable.

[0174] At the same time, the nanohardness of the high-order electrostatic dissipative carbon-based multi-composite film material prepared in this application reaches 1600HV-2000HV, and the friction coefficient is 0.05-0.15. These two performance indicators are far superior to traditional coating materials, thereby enhancing wear resistance and extending service life.

[0175] For example, the characteristics of conventional amorphous diamond-like carbon-based film materials (aC:H) are: high film hardness, good self-lubricating properties, and strong wear resistance, but they cannot meet other performance indicators, such as: impedance values ​​within a specific range, high chemical stability and thermal stability, and anti-adhesion performance. Based on the above comprehensive performance requirements, the research direction here is to improve and optimize the composition and structure of the original material by adding multiple other elements to the existing carbon element film material, so as to prepare a new type of multi-component composite material.

[0176] It should be noted that when selecting raw materials, silicon (Si) and oxygen (O) elements are first doped to study the changes in the structure and performance of the materials. After adding silicon (Si) and oxygen (O) to the conventional material aC:H, a small part of the carbon atoms in the film layer are replaced by silicon atoms and oxygen atoms, and the structure of the new material has changed a little. In addition to the amorphous aC:H structure, an amorphous a-Si:O structure is formed, such as Figure 2 As shown, a schematic diagram of the structure of a quaternary carbon-based thin film composite material containing carbon, hydrogen, silicon and oxygen is shown. Due to the reduction of sp3 hybrid bonds, the hardness of the film layer is slightly reduced, and the nanohardness value is reduced from the original 2300HV to around 2000HV.

[0177] Secondly, due to the presence of oxygen-containing amorphous silicon structure, the material's oxidation resistance and thermal stability are improved to a certain extent. Figure 3 As shown in the figure, a comparison chart of the surface energies of aC:H and aC:H:Si:O materials is shown. When water is dropped on the surfaces of two different materials, two different phenomena can be seen. The contact angle R2 between the water droplet and the surface of the aC:H:Si:O material is greater than the angle R1 with the surface of the aC:H material. The surface energy measurement confirms that the surface energy of the aC:H:Si:O material is about 10mH / m lower than that of the original material. This shows that silicon-doped and oxygen-doped materials have excellent anti-adhesion properties.

[0178] In addition, the resistance test results show that after adding these two elements, the surface resistance of the material is 10 9 -10 14 ohms range, which has not yet reached the ESD protection standard for device components defined in the JEDEC standard. In order to meet the range requirements of controllable resistance, the composition of the material needs to be further improved. We also added three elements, silicon (Si), oxygen (O), and titanium (Ti), and tested the performance.

[0179] For example, after adding a third metal element, titanium (Ti), a third amorphous titanium chain structure appears in the five-element carbon-based film material, such as Figure 4 As shown, a schematic diagram of the structure of a five-element carbon-based thin film composite material containing carbon, hydrogen, silicon, oxygen and titanium is shown. Experimental data show that the surface resistance value of the new carbon-based five-element composite material aC:H:Si:O:Ti in the present application is determined by the amount of titanium element component, such as Figure 5 As shown, the relationship between the surface resistance value of the film layer and the titanium atom content is shown.

[0180] For example, Table 1 lists the one-to-one correspondence between the surface resistance value of the new material and the percentage of titanium atoms. A series of experimental data show that when the percentage of titanium atoms is between 1.0-2.0%, the surface resistance value range can be controlled within 10 5 -10 9 ohms, thus meeting special requirements.

[0181] Table 1 Correspondence between surface resistance value and titanium atomic percentage

[0182] Titanium atomic percentage [%] Surface resistance [ohms] 0 <![CDATA[1.1x10 14 ]]> 0.2 <![CDATA[5.1x10 13 ]]> 0.4 <![CDATA[5.0x10 12 ]]> 0.6 <![CDATA[8.8x10 10 ]]> 0.8 <![CDATA[2.9x10 10 ]]> 1.0 <![CDATA[1.2x10 9 ]]> 1.2 <![CDATA[3.0x10 8 ]]> 1.4 <![CDATA[8.3x10 7 ]]> 1.6 <![CDATA[5.8x10 6 ]]> 1.8 <![CDATA[5.3x10 5 ]]> 2.0 <![CDATA[1.9x10 5 ]]> 2.5 <![CDATA[8.7x10 4 ]]> 3 <![CDATA[5.1x10 3 ]]> 4 <![CDATA[1.8x10 3 ]]> 5 <![CDATA[1.5x10 3 ]]>

[0183] Performance Test:

[0184] After determining the final doping elements and their composition ratios of the material, the friction coefficient of the prepared new film material was tested using a friction and wear tester (Pin-on-Disc). The test results showed that the dry friction coefficient of this material against stainless steel was between 0.05-0.15, which belongs to the category of super-lubricating materials. To improve wear resistance, the nano-hardness and surface roughness of the film material are also critical. The nano-hardness of the product is measured according to the DIN EN ISO 14577-1 standard, such as Figure 6 As shown, the product nano-hardness measurement curve is shown. The product nano-hardness measurement curve shows that the hardness value ranges from 1600-2000HV. Using the German Mahr roughness measuring instrument, it is found that the roughness value of the product is between Ra0.1-0.2 when the film thickness is 3-5 microns.

[0185] On the other hand, the film thickness was measured to be between 3 and 5 microns by ball mill plus microscope. Figure 7 As shown, the measurement results of the film thickness of the present application are shown. For the film thickness, the bonding strength between the film material and the substrate material is very important. This index is detected by a Rockwell hardness tester using a 150 kg dot method, such as Figure 8 As shown in the figure, it shows the standard diagram for judging the film bonding strength. The judging standard is based on the German standard VDI3198. HF1 to HF4 are good film bonding strengths recognized by the industry standard, and H5-H6 are poor. This product reaches the HF1 level. Fig. 9 As shown, the bonding force diagram of this product is shown. In addition, the surface energy value of this material also reaches 23-30mN / m, which is 10mN lower than that of conventional diamond-like carbon film material aC.

[0186] At the same time, similar products on the market (comparative example) and the high-order electrostatic dissipative carbon-based multi-component composite film material prepared in this application (Example 5) were taken for performance comparison. The performance comparison results are shown in Table 2.

[0187] Table 2 Performance comparison table

[0188]

[0189]

[0190] In summary, the material provided by the present invention adopts two different mixed vapor deposition technologies, namely, advanced anode layer ion source and unbalanced magnetron sputtering. By adding silicon, oxygen and titanium elements to the existing amorphous carbon-based thin film materials, special process parameters are developed to prepare special multi-component composite materials with improved composition and structure, thereby meeting the comprehensive material performance requirements customized by customers.

[0191] The antistatic resistance value of the high-order electrostatic dissipative carbon-based multi-component composite film material prepared in this application is precisely controlled within 10 5 -10 9 It is within the range of 0.1 ohms and meets the industry testing standards of JEDEC-JESD625B. It has chemical stability and temperature resistance. The film layer will not peel off at low temperatures of -50°C to high temperatures of 200°C, and the surface resistance value can remain stable.

[0192] At the same time, the nanohardness of the high-order electrostatic dissipative carbon-based multi-component composite film material prepared in this application reaches 1600HV-2000HV, and the friction coefficient is 0.05-0.15. These two performance indicators are far superior to traditional coating materials, thereby enhancing wear resistance and extending service life. At the same time, it has good surface anti-adhesion effect, and its surface energy is in the lower range of 23-30mN / m; it also has a lower surface roughness: Ra 0.1-0.2.

[0193] It should be noted that, for the above-mentioned embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.

[0194] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. High-order electrostatic dissipative carbon-based multi-component composite film material, characterized in that: The high-order electrostatic dissipative carbon-based multi-component composite thin film material is prepared by using two different mixed gas phase deposition technologies: anode layer ion source and unbalanced magnetron sputtering; Among them, the anode layer ion source technology is used to prepare an ultra-wear-resistant diamond-like carbon-based thin film material with high hardness, low friction coefficient and fine surface. The unbalanced magnetron sputtering technology is used to adjust the power of the magnetron sputtering to ensure that a specific amount of element composition ratio is modulated, thereby facilitating the addition of alloy elements; The high-level electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: carbon element 72-78%, silicon element 12-18%, oxygen element 5-10%, titanium element 0.5-3.5%; The high-order electrostatic dissipative carbon-based multi-component composite film material is added with three different elements, silicon, oxygen and titanium, and is a high-order multi-component film composite material containing carbon, hydrogen, silicon, oxygen and titanium aC:H:Si:O:Ti, and has a variety of composite structures; The structure of high-order electrostatic dissipative carbon-based multi-component composite film materials includes: sp2 graphite phase structure; sp3 diamond phase structure, among which sp2 graphite phase structure and sp3 diamond phase structure are the basic structures of the original materials; The second amorphous silicon-oxygen a-Si:O structure is formed after doping with silicon and oxygen; The third amorphous titanium chain a-Ti structure formed by adding titanium element; The nano-hardness of the high-order electrostatic dissipative carbon-based multi-component composite film material is 1600HV-2000HV, the friction coefficient is 0.05-0.15, and the anti-static resistance value of the film layer is 10 5 -10 9 ohms, surface roughness is Ra0.1-0.2; The method for preparing the high-order electrostatic dissipative carbon-based multi-component composite film material specifically comprises: Step S10, obtaining raw materials for preparing the multi-component composite thin film material, placing the raw materials into the coating chamber, and pre-treating the raw materials; Step S20, in the coating preparation stage, the raw materials are coated with titanium base layer, transition layer and functional layer respectively by using an anode layer ion source and unbalanced magnetron sputtering technology; Step S30, cooling treatment after coating, closing all parameter settings, the rotating frame continues to maintain 4 revolutions per minute, cooling to 120° C. and then opening the furnace to obtain a carbon-based multi-component composite film material with electrostatic dissipation function; The method of obtaining raw materials for preparing multi-component composite thin film materials, placing the raw materials into a coating chamber, and pre-treating the raw materials specifically includes: Step S101, taking raw materials for preparing multi-component composite thin film materials; Step S102, turning on the turntable to draw the vacuum degree in the chamber to 0.05 Pa, wherein the turntable is set to rotate at 4 rpm; Step S103, turning on the two heat radiation heating plates at the same time, heating at a constant temperature continuously and then turning off the heating plates, wherein the thermocouple temperature control value is set to 120°C, and heating at a constant temperature continuously for 30 minutes and then turning off the heat radiation heating plates; Step S104, introducing argon gas, setting the flow rate of the introduced argon gas to 250 sccm, turning on the two anode layer ion sources, setting their voltages to 1200 V, applying a bias voltage of 800 V, a pulse frequency of 40 kHz and a duty cycle of 20% to the workpiece, and performing an ion etching and cleaning process for 60 minutes; In the coating preparation stage, the method of coating the raw materials with titanium base layer, transition layer and functional layer respectively by using anode layer ion source and unbalanced magnetron sputtering technology specifically includes: Step S201, titanium base layer preparation, close the anode layer ion source, open the baffles of the two rows of titanium targets, adjust the argon flow rate to 50-150sccm, set the sputtering power of the titanium target to 5-20kW, load the bias voltage to 500-1200V, the pulse frequency to 10-150kHz and the duty cycle to 5-50%, and continue titanium plating for 10 minutes; Step S202, continue sputtering titanium, adjust the argon flow rate to 50-150 sccm, the target power to 5-20 kW, and introduce acetylene at a flow rate of 100-350 sccm, and the transition layer lasts for 30 minutes; Step S203, keep the magnetron sputtering titanium working, adjust the power to 5-20kW, turn on the anode layer ion source, set the voltage to 500-1500V, introduce acetylene flow rate 250sccm and hexamethyldisiloxane 2-10g / min, load bias to 500-1200V, pulse frequency 10-150kHz and duty cycle 5-50%, and deposition time is 250 minutes.

2. The high-order electrostatic dissipative carbon-based multi-component composite film material according to claim 1, characterized in that: The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: carbon element 74-76%, silicon element 14-16%, oxygen element 6-8%, and titanium element 0.8-3%.

3. The high-order electrostatic dissipative carbon-based multi-component composite film material according to claim 2, characterized in that: The high-order electrostatic dissipative carbon-based multi-component composite film material includes the following raw materials in percentage: 75% carbon element, 15% silicon element, 7% oxygen element, and 2% titanium element.

Citation Information

Patent Citations

  • Ti / Si co-doped ta-C conductive carbon-based thin film and preparation method and application thereof

    CN115058696A

  • Novel silicon-containing oxygen-containing high-order static dissipation film composite material and preparation method thereof

    CN115612989A

  • Wear-resistant carbon-based composite film for aerospace sealing element and preparation method of wear-resistant carbon-based composite film

    CN117070893A

  • Method for forming diamond-like nanocomposite or doped-diamond-like nanocomposite films

    US5352493A