A method for accurately controlling the polishing thickness of silicon wafers for integrated circuits
By dynamically adjusting the polishing pressure and temperature, the problem of inconsistent thickness of single crystal silicon wafers is solved, the polishing efficiency and thickness uniformity are improved, and the customer's thickness requirements are met.
Patent Information
- Application Number
- CN202110723046.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-06-29
AI Technical Summary
During the chemical mechanical polishing process of single crystal silicon wafers, since the polishing pressure and temperature are constant values, the thickness of the silicon wafers is inconsistent, which affects product quality, and the polishing efficiency is low, making it difficult to process silicon wafers with large thickness differences, especially in small batches. In production.
By dynamically adjusting the polishing pressure and temperature according to the thickness difference of the incoming single crystal silicon wafers, the removal rate of silicon wafers with larger thickness is increased and the removal rate of silicon wafers with smaller thickness is reduced, ensuring the consistency of thickness after polishing and shortening the polishing time. time.
It achieves the uniformity and consistency of silicon wafer thickness, improves polishing efficiency, meets the thickness uniformity required by customers, and significantly shortens polishing time.
Smart Images

Figure CN115533733B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of integrated circuit silicon wafer production, and in particular to a method for accurately controlling the polishing thickness of an integrated circuit silicon wafer. Background Art
[0002] Semiconductor silicon materials are the main functional materials of the electronic information industry, especially the integrated circuit industry. As the diameter of silicon wafers becomes larger and the feature size of integrated circuits becomes smaller, higher technical requirements are placed on the overall performance of single-crystal silicon wafers, among which the thickness consistency of single-crystal silicon wafers is a key technical indicator. In the processing of single-crystal silicon wafers, double-sided chemical mechanical polishing, as one of the most effective technical means for ultra-smooth surface processing of silicon wafers, has received extensive attention and attention in the field of ultra-precision processing research and semiconductor silicon material production and processing companies. The total amount of material removed by double-sided chemical mechanical polishing of single-crystal silicon wafers is the sum of the amount of material removed by chemical action, mechanical action, and the amount of material removed by the mutual promotion of chemical and mechanical action. The polishing pressure and polishing temperature have a significant effect on the removal rate of silicon wafers. In the conventional chemical mechanical polishing process, constant polishing pressure and polishing temperature are often used to ensure that the mechanical grinding speed and chemical corrosion speed are basically consistent. Since the polishing pressure and polishing temperature during the polishing process are constant, the removal rate of silicon wafer materials tends to be uniform. However, due to the difference in thickness of each single crystal silicon wafer on the same polishing disk, when the thickness difference of each single crystal silicon wafer exceeds a certain value, grinding deviation will occur, resulting in various quality problems that affect product consistency, such as inconsistent local flatness of the single crystal silicon wafer after polishing and poor thickness consistency. In order to solve this problem and ensure the uniformity of the thickness of the silicon wafer after polishing, the aforementioned method has very high requirements for the thickness range of the incoming materials for polishing the same batch of silicon wafers, which is usually controlled within 2μm. A lot of time is required in the incoming material thickness grading stage before polishing, and the overall polishing efficiency is low, which is the bottleneck link in the production capacity of the entire silicon wafer manufacturing process. Small batches of products cannot be processed, which seriously affects production capacity, especially the promotion of products in the process of sample delivery and certification.
[0003] In order to solve the above technical problems, the present invention provides a method for accurately controlling the polishing thickness of silicon wafers for integrated circuits. According to the change in the amount of material removed from the single crystal silicon wafer during the chemical mechanical polishing process, the polishing pressure and polishing temperature during the polishing process are continuously adjusted to control the thickness, thereby increasing the removal rate of thicker silicon wafers and reducing the removal rate of thinner silicon wafers, ensuring the consistency of the thickness of the silicon wafers after polishing, and at the same time shortening the polishing time and improving the overall polishing efficiency. Summary of the invention
[0004] In order to achieve the above requirements, the object of the present invention is to provide a method for accurately controlling the thickness of chemical mechanical polishing of silicon wafers for integrated circuits, comprising the following steps:
[0005] The first step is to determine the thickness range of the same group of polished single crystal silicon wafers according to the technical requirements of the internal control standard for single crystal silicon wafers. spec , the scope of application of the present invention is Diff spec =1~2μm;
[0006] The second step is to determine the thickness range Diff of the same group of polished single crystal silicon wafers according to the empirical equation (1). wafer ,
[0007] Diff wafer =D max -D min (1)
[0008] Where D max is the maximum thickness of the single crystal silicon wafers polished in the same group, D min The minimum thickness of the incoming single crystal silicon wafers polished in the same group;
[0009] Diff wafer The suitable range of is consistent with the empirical equation (2):
[0010] Diff spec ≤Diff wafer ≤1.5Diff spec (2)
[0011] When Diff wafer =1.5Diff spec When the maximum value of the thickness range of the same group of polished single crystal silicon wafers is determined, it is recorded as: Diff wafer,max ;
[0012] The third step is to measure and calculate the average thickness of the incoming single crystal silicon wafers of the same group of polished wafers, recorded as D0, and determine the target thickness value of the silicon wafer after polishing according to the internal control standard requirements, recorded as D spec The pressure P during the polishing process is determined according to the empirical equation (3):
[0013]
[0014] Where: K is the pressure coefficient, and the value in the patent method of the present invention is: K = 1.71; P min is the minimum pressure.
[0015] It can be seen that according to the empirical equation (3), the pressure is relatively high when polishing just starts. As polishing progresses, the polishing pressure P decreases with the decrease in the thickness of the single crystal silicon wafer. According to the principle of mechanical polishing, the higher the pressure, the faster the grinding and removal of thicker silicon wafers is than that of thinner single crystal silicon wafers. This can effectively reduce the thickness range of the same group of polished single crystal silicon wafers and improve the thickness uniformity and consistency.
[0016] In the fourth step, the temperature during the polishing process is determined according to the empirical equation (4):
[0017]
[0018] Where: L is the temperature coefficient, and the value in the patent method of the present invention is: L = 0.29; T min is the minimum temperature.
[0019] It can be seen that according to equation (4), the temperature is relatively high when polishing just starts. As polishing proceeds, the polishing temperature T decreases as the thickness of the single crystal silicon wafer decreases. According to the principle of chemical corrosion, higher temperatures cause greater polishing pressure and strain on thicker silicon wafers, resulting in a much faster removal rate than that of thinner single crystal silicon wafers, further effectively reducing the thickness range of the same group of polished single crystal silicon wafers and improving thickness uniformity and consistency.
[0020] In the patented technology of this invention, it is required that at the minimum pressure P min and minimum temperature T min Under these conditions, the mechanical polishing removal rate is close to the chemical etching polishing removal rate, which conforms to equation (5):
[0021]
[0022] In the formula, K is 11.3, Ea is the activation energy of the corrosion reaction; R is the molar gas constant;
[0023] When Diff wafer <Diff spec When the minimum pressure P is constant, min and minimum temperature T min Polishing conditions.
[0024] The thickness of the polished silicon wafers produced by the patented invention can be controlled within the range required by the customer's Spec, the thickness uniformity is significantly improved, and the polishing time is greatly shortened. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the curve of polishing pressure changing with polishing removal amount.
[0026] Figure 2 It is the curve of polishing temperature changing with polishing removal amount. DETAILED DESCRIPTION
[0027] Example 1
[0028] Polishing 300mm silicon wafers, according to the technical requirements of the internal control standard for monocrystalline silicon wafers, the thickness range of the incoming monocrystalline silicon wafers of the same group of polishing is 2.0μm; the maximum value of the incoming thickness of the monocrystalline silicon wafers of the same group of polishing is 789.5μm, the minimum value is 786.5μm, and the average value is 787.48μm. According to equation (1), the thickness range is 3.0μm; satisfying equation (2), and then according to equation (3), the initial value of the polishing pressure is determined to be 12.86kpa, and it is continuously adjusted according to equation (3); according to equation (4), the initial value of the polishing temperature is determined to be 24.64℃, and it is continuously adjusted according to equation (4). 45 300mm silicon wafers were polished with this process, and the thickness range of the polished monocrystalline silicon wafers was 1.0μm, and the polishing time was 230 minutes, which met the customer's Spec requirements.
[0029] Comparative Example 1
[0030] Polishing 300 mm silicon wafers, according to the technical requirements of the internal control standard for single crystal silicon wafers, the thickness range of the single crystal silicon wafers polished in the same group is 2.0 μm; the maximum value of the thickness of the single crystal silicon wafers polished in the same group is 788.5 μm, the minimum value is 786.5 μm, and the average value is 787.48 μm. According to equation (1), the thickness range is 2.0 μm; 45 300 mm silicon wafers are polished at a constant pressure and temperature. The thickness range of the polished single crystal silicon wafers is 1.0 μm, which is similar to the result of Example 1. The polishing time is 278 minutes, which is longer than that of Example 1 and meets the customer's Spec requirements.
[0031] Example 2
[0032] Polishing 300mm silicon wafers, according to the technical requirements of the internal control standard for monocrystalline silicon wafers, the thickness range of the same group of monocrystalline silicon wafers is 1.0μm; the maximum value of the thickness of the same group of monocrystalline silicon wafers is 780.3μm, the minimum value is 778.8μm, and the average value is 779.52μm. According to equation (1), the thickness range is 1.5μm; satisfying equation (2), and then according to equation (3), the initial value of the polishing pressure is determined to be 6.62kpa, and it is adjusted continuously according to equation (3); according to equation (4), the initial value of the polishing temperature is determined to be 23.60℃, and it is adjusted continuously according to equation (4). 45 300mm silicon wafers are polished with this process, and the thickness range of the polished monocrystalline silicon wafers is 0.7μm, which meets the customer's Spec requirements.
[0033] Example 3
[0034] Polishing 300mm silicon wafers, according to the technical requirements of the internal control standard for monocrystalline silicon wafers, the thickness range of the incoming monocrystalline silicon wafers of the same group of polishing is 1.2μm; the maximum value of the incoming thickness of the monocrystalline silicon wafers of the same group of polishing is 783.6μm, the minimum value is 781.8μm, and the average value is 782.02μm. According to equation (1), the thickness range is 1.8μm; satisfying equation (2), and then according to equation (3), the initial value of the polishing pressure is determined to be 7.50kpa, and it is continuously adjusted according to equation (3); according to equation (4), the initial value of the polishing temperature is determined to be 23.75℃, and it is continuously adjusted according to equation (4). 45 300mm silicon wafers are polished with this process, and the thickness range of the polished monocrystalline silicon wafers is 0.9μm, which meets the customer's Spec requirements.
[0035] Example 4
[0036] Polishing 300mm silicon wafers, according to the technical requirements of the internal control standard for monocrystalline silicon wafers, the thickness range of the same group of monocrystalline silicon wafers is 1.2μm; the maximum value of the thickness of the same group of monocrystalline silicon wafers is 782.7μm, the minimum value is 781.9μm, and the average value is 782.28μm. According to equation (1), the thickness range is 0.8μm; if equation (2) is not satisfied, the minimum pressure and temperature are calculated according to equation (5), and polishing is performed with constant minimum pressure and temperature. 45 300mm silicon wafers are polished with this process, and the thickness range of the polished monocrystalline silicon wafers is 1.0μm, which meets the customer's Spec requirements.
Claims
1. A method for accurately controlling the thickness of chemical mechanical polishing of silicon wafers for integrated circuits, according to the extreme value of incoming thickness difference of single crystal silicon wafers required by internal control standards, determining the maximum extreme value of incoming thickness difference of single crystal silicon wafers polished in the same group; continuously adjusting the polishing pressure during the polishing process by a pressure calculation equation; continuously adjusting the polishing temperature during the polishing process by a temperature calculation equation; when the extreme value of incoming thickness difference of single crystal silicon wafers polished in the same group is less than the extreme value of incoming thickness difference of single crystal silicon wafers required by internal control standards, selecting constant minimum pressure and minimum temperature that meet the condition that the mechanical grinding polishing removal rate and the chemical etching polishing removal rate are close to each other for polishing, until the target thickness value of the silicon wafer after polishing required by the customer is reached; characterized in that The following steps are involved: The first step is to determine the thickness difference of the same group of polished single crystal silicon wafers required by the internal control standard. spec ; The second step is to calculate the thickness difference of the same group of polished single crystal silicon wafers. wafer According to equation (1), Diff wafer =D max -D min (1) Where D max is the maximum thickness of the single crystal silicon wafers polished in the same group, D min The minimum thickness of the incoming single crystal silicon wafers polished in the same group; Diff wafer The range of is consistent with equation (2): Diff spec ≤Diff wafer ≤1.5Diff spec (2) In the third step, the pressure P during the polishing process conforms to equation (3): Where: K is the pressure coefficient, the value is: K = 1.71; P min is the minimum pressure; D0 is the average thickness of the single crystal silicon wafers polished in the same group; D spec Determine the target thickness of the silicon wafer after polishing for internal control standard requirements; In the fourth step, the temperature during the polishing process conforms to equation (4): Where: L is the temperature coefficient, the value is: L = 0.29; T min is the minimum temperature; D0 is the average thickness of the single crystal silicon wafers polished in the same group; D spec Determine the target thickness value of the silicon wafer after polishing for internal control standard requirements.
2. The method for accurately controlling the thickness of chemical mechanical polishing of silicon wafers for integrated circuits according to claim 1, characterized in that: At the minimum pressure P min and minimum temperature T min Under these conditions, the mechanical polishing removal rate is close to the chemical etching polishing removal rate, which conforms to equation (5): In the formula, K is 11.3, Ea is the activation energy of the corrosion reaction; R is the molar gas constant.
3. The method for accurately controlling the thickness of chemical mechanical polishing of silicon wafers for integrated circuits according to claim 1, characterized in that: When Diff wafer <Diff spec When the minimum pressure P is constant, min and minimum temperature T min Polishing conditions.
4. The method for accurately controlling the thickness of chemical mechanical polishing of silicon wafers for integrated circuits according to claim 1, characterized in that: The thickness difference of the same group of polished single crystal silicon wafers required by the internal control standard is Diff. spec The range is: Diff spec =1~2μm.
Citation Information
Patent Citations
Polishing method for silicon wafer
CN105252406A
Polishing equipment and polishing pressure control method and device thereof
CN107336126A
Chemical mechanical polishing method and chemical polishing system
CN110193775A
Method for controlling thickness of polished heavily-doped product
CN111203792A
Chemical mechanical polishing method, device and system and control equipment
CN111863613A
Cited By
Silicon wafer V-shaped groove polishing positioning deviation management and control system
CN122008061A