Collagen fiber-based foaming material and preparation method and application thereof
By using tannin modified collagen fibers in water-based polyurethane for foaming, the problems of low strength and flammability of water-based polyurethane foaming materials are solved, the mechanical, thermal insulation and flame retardant properties are improved, and solid waste resource utilization is realized , improves the comprehensive performance and environmental protection of the materials.
Patent Information
- Application Number
- CN202211325997.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-27
AI Technical Summary
The low strength and flammability of existing water-based polyurethane foaming materials limit their application, and other performance and cost defects will be introduced when improving various properties by adding functional fillers.
The mixture of tannin modified collagen fibers and aqueous polyurethane is used for foaming and molding. By improving interface compatibility and the support of bubble cells, the mechanical properties, thermal insulation properties and flame retardant properties of foamed materials are improved.
The high mechanical properties, thermal insulation properties and flame retardant properties of collagen fiber-based foamed materials are achieved, and solid waste resource utilization is realized through the addition of functional materials, improving the multi-party performance and green environmental protection of the materials.
Smart Images

Figure CN115584118B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a collagen fiber-based foaming material and a preparation method and application thereof. Background Art
[0002] Waterborne polyurethane foam is an important synthetic material with the characteristics of light weight, high elasticity, sound absorption, and breathability. It can be made into soft, hard, and semi-hard foam materials according to the different raw materials and formulas used. It is widely used in papermaking, construction, packaging, automotive industry, etc. Among them, the soft waterborne polyurethane foam with an open-cell structure is limited in application due to its low strength, low porosity, flammability, and other problems.
[0003] In the prior art, the performance of waterborne polyurethane foaming materials is improved by adding functional fillers, for example, nanoparticles and glass fibers are used for reinforcement, and flame retardants such as magnesium-aluminum hydrotalcite, organic clay and melamine are used to improve their flame retardancy. However, if multiple performances of waterborne polyurethane foaming materials are to be improved, multiple functional fillers need to be added, and at the same time, too much filler addition will introduce other performance and cost defects.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One object of the present invention is to provide a method for preparing a collagen fiber-based foam material to solve the technical problems of low strength and flammability of waterborne polyurethane foam materials in the prior art.
[0006] Another object of the present invention is to provide a collagen fiber-based foam material having excellent mechanical properties, thermal insulation properties and flame retardant properties.
[0007] Another object of the present invention is to provide application of collagen fiber-based foaming material in sound insulation and heat preservation material.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The preparation method of the collagen fiber-based foaming material comprises the following steps:
[0010] The mixture of tannin modified collagen fiber and waterborne polyurethane is foamed and formed to obtain collagen fiber-based foaming material.
[0011] The tannin modified collagen fiber used in the present invention has good dispersibility in waterborne polyurethane, improves the interfacial compatibility with the waterborne polyurethane matrix, is conducive to the formation of foam cores, and plays a supporting and stabilizing role on the formed pores, thereby improving the porosity of the obtained foam material, and improving the mechanical properties and thermal insulation properties of the foam material. The tannin modified collagen fiber of the present invention can ensure that the fiber is better dispersed in the foam material, and play a skeleton supporting role of the collagen fiber in the foam material.
[0012] In a specific embodiment of the present invention, in the mixture, the tannin modified collagen fiber accounts for 1wt% to 30wt%.
[0013] In a specific embodiment of the present invention, the foaming includes any one or more combinations of mechanical foaming, physical foaming and chemical foaming.
[0014] In a specific embodiment of the present invention, the mechanical foaming method includes mechanical stirring foaming; the physical foaming method includes foaming using a physical foaming agent; and the chemical foaming method includes foaming using a chemical foaming agent.
[0015] In a specific embodiment of the present invention, the physical foaming agent includes any one or more of sodium dodecyl sulfonate, sodium dodecyl sulfate and sodium tetradecyl sulfonate; the chemical foaming agent includes any one or more of azodicarbonamide, diethyl azodicarboxylate and p-toluenesulfonyl hydrazide.
[0016] In a specific embodiment of the present invention, in the mechanical stirring foaming, the stirring speed is 2500-3500 r / min; and the stirring time is 1-10 min.
[0017] In a specific embodiment of the present invention, the molding comprises: drying and molding in a mold. Furthermore, the drying temperature is 80-120°C.
[0018] In a specific embodiment of the present invention, the tannin-modified collagen fiber is a plant tannin-modified collagen fiber, wherein the plant tannin is a condensed tannin or a mixed tannin; the plant tannin includes any one or more of the following: bayberry tannin, black wattle tannin, larch tannin, quebracho tannin, and acacia mangium tannin.
[0019] In a specific embodiment of the present invention, the tannin-modified collagen fiber is bayberry tannin-modified collagen fiber.
[0020] The present invention also provides a collagen fiber-based foam material prepared by using any one of the above methods for preparing a collagen fiber-based foam material.
[0021] In a specific embodiment of the present invention, the tensile strength of the collagen fiber-based foaming material is ≥1.2MPa, and the fracture energy is ≥650KJ / m 3 , limiting oxygen index ≥ 20%, porosity ≥ 50%.
[0022] The present invention also provides the use of any one of the above-mentioned collagen fiber-based foaming materials as a sound insulation and heat preservation material.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The tannin-modified collagen fiber used in the present invention has good dispersibility in waterborne polyurethane, improves the interfacial compatibility with the waterborne polyurethane matrix, is conducive to the formation of foam cores, and plays a supporting and stabilizing role for the formed pores, thereby improving the porosity of the obtained foam material, and improving the mechanical properties, flame retardant properties, thermal insulation properties, etc. of the polyurethane foam material;
[0025] (2) The present invention uses tannin-modified collagen fibers as functional materials and adds them into the waterborne polyurethane matrix. On the one hand, it realizes the resource utilization of solid waste. On the other hand, it greatly improves the various properties of the waterborne polyurethane foaming material, achieving high-value utilization, greenness, and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The tensile stress-strain curves and fracture energies of the materials prepared in the embodiments of the present invention and the comparative examples;
[0028] Figure 2 This is a FESEM photograph of the tensile fracture surface of the WPUF / BT-LCF prepared in Example 1 of the present invention;
[0029] Figure 3 is the limiting oxygen index of the WPUF of the present invention and WPUF / LCF, WPUF / DLCF, WPUF / BT-LCF, and WPUF / BT-DLCF with different collagen fiber contents;
[0030] Figure 4Infrared thermal imaging images of four composite materials, namely, WPUF / BT-LCF prepared in Example 1 of the present invention, WPUF / LCF prepared in Comparative Example 1, WPUF / DLCF prepared in Comparative Example 2, and WPUF / BT-DLCF prepared in Comparative Example 3; wherein a to d are WPUF / LCF, WPUF / DLCF, WPUF / BT-LCF, and WPUF / BT-DLCF, respectively. DETAILED DESCRIPTION
[0031] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0032] The preparation method of the collagen fiber-based foaming material comprises the following steps:
[0033] The mixture of tannin modified collagen fiber and waterborne polyurethane is foamed and formed to obtain collagen fiber-based foaming material.
[0034] The natural multi-level micro / nano structure of collagen fiber is essentially a multi-level pore structure, which can play a role of supporting pores in waterborne polyurethane, so the introduction of collagen fiber can improve the porosity and pore stability of waterborne polyurethane. The tannin-modified collagen fiber used in the present invention has good dispersibility in waterborne polyurethane, improves the interface compatibility with the waterborne polyurethane matrix, is conducive to the formation of bubble cores, and plays a supporting and stabilizing role on the formed pores, thereby improving the porosity of the obtained foaming material, and improving the mechanical properties and thermal insulation properties of the foaming material.
[0035] In actual operation, the waterborne polyurethane may be an anionic waterborne polyurethane, or may be a cationic waterborne polyurethane or a nonionic waterborne polyurethane.
[0036] In a specific embodiment of the present invention, in the mixture, the tannin modified collagen fiber accounts for 1wt% to 30wt%.
[0037] For example, in different embodiments, in the mixture, the proportion of tannin-modified collagen fibers can be 1wt%, 2wt%, 5wt%, 8wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% and the like.
[0038] In a specific embodiment of the present invention, in the mixture, the tannin-modified collagen fibers account for 5wt% to 25wt%, preferably 20wt% to 25wt%.
[0039] In a specific embodiment of the present invention, the foaming includes any one or more combinations of mechanical foaming, physical foaming and chemical foaming.
[0040] In a specific embodiment of the present invention, the mechanical foaming method includes mechanical stirring foaming; the physical foaming method includes foaming using a physical foaming agent; and the chemical foaming method includes foaming using a chemical foaming agent.
[0041] In a specific embodiment of the present invention, the physical foaming agent includes any one or more of sodium dodecyl sulfonate, sodium dodecyl sulfate and sodium tetradecyl sulfonate; the chemical foaming agent includes any one or more of azodicarbonamide, diethyl azodicarboxylate and p-toluenesulfonyl hydrazide.
[0042] In a specific embodiment of the present invention, in the mechanical stirring foaming, the stirring speed is 2500-3500 r / min; and the stirring time is 1-10 min.
[0043] For example, in different embodiments, the stirring speed can be 2500r / min, 2600r / min, 2800r / min, 3000r / min, 3200r / min, 3400r / min, 3500r / min, etc.; the stirring time can be 1min, 2min, 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min, etc.
[0044] In a specific embodiment of the present invention, the molding comprises: drying and molding in a mold. Furthermore, the drying temperature is 80-120°C.
[0045] In actual operation, the mixture can be poured into a polytetrafluoroethylene mold and placed in an oven until it is dried.
[0046] In a specific embodiment of the present invention, the tannin-modified collagen fiber is a plant tannin-modified collagen fiber, wherein the plant tannin is a condensed tannin or a mixed tannin; the plant tannin includes any one or more of the following: bayberry tannin, black wattle tannin, larch tannin, quebracho tannin, and acacia mangium tannin.
[0047] In a specific embodiment of the present invention, the tannin-modified collagen fiber is bayberry tannin-modified collagen fiber.
[0048] In a specific embodiment of the present invention, the preparation of the tannin modified collagen fiber comprises: mixing tannin and collagen fiber in a liquid environment with a pH of 5 to 6, followed by washing and drying.
[0049] In a specific embodiment of the present invention, the mass ratio of the tannin to the collagen fiber is 1:(1-10), preferably 1:(2-5), and further 1:(3-4).
[0050] In actual operation, after the aqueous solution of tannin is mixed with the aqueous dispersion of collagen fibers, the pH is adjusted to 5-6 with alkali, and the mixture is stirred for 4-6 hours and then filtered. The solid is washed with ethanol to remove unreacted tannin, and then dried at 65-85°C for 18-24 hours to obtain tannin-modified collagen fibers.
[0051] The collagen fibers in the raw material can be obtained by pre-treating waste leather scraps. Waste leather scraps include metal tanned waste leather scraps, such as blue leather scraps. The pre-treatment includes: dehydrating and crushing the waste leather scraps. The dehydration method can be adjusted and selected according to actual needs, such as any one or more of natural drying, heating drying, ethanol dehydration, freeze drying and vacuum drying.
[0052] In a specific embodiment of the present invention, the preparation of the collagen fiber includes: dispersing waste leather scraps in water, adjusting the pH to 5-7, filtering and dehydrating with ethanol, drying and crushing after the ethanol evaporates to obtain collagen fibers.
[0053] The present invention also provides a collagen fiber-based foam material prepared by using any one of the above methods for preparing a collagen fiber-based foam material.
[0054] In a specific embodiment of the present invention, the tensile strength of the collagen fiber-based foaming material is ≥1.2MPa, and the fracture energy is ≥650KJ / m 3 , limiting oxygen index ≥ 20%, porosity ≥ 50%.
[0055] For example, in different embodiments, the tensile strength of the collagen fiber-based foaming material is ≥1.2MPa, ≥1.25MPa, ≥1.3MPa, ≥1.35MPa, etc.; the fracture energy is ≥650KJ / m 3 ,≥660KJ / m 3 ,≥670KJ / m 3 ,≥680KJ / m 3 ,≥690KJ / m 3 , ≥700KJ / m 3 Etc.; Limiting oxygen index ≥20%, ≥21%, ≥22%, ≥23%, ≥24%, etc.; Porosity ≥50%, ≥55%, ≥60%, ≥65%, etc.
[0056] The present invention also provides the use of any one of the above-mentioned collagen fiber-based foaming materials as a sound insulation and heat preservation material.
[0057] Some of the substance information used in the specific embodiments of the present invention may be as follows:
[0058] Blue leather shavings, sourced from Haining Ruixing Leather Co., Ltd.;
[0059] Anionic water-based polyurethane, Hefei Ketian Water-based Technology Co., Ltd.; but not limited to this.
[0060] The collagen fibers used in the following specific embodiments can be prepared from blue leather scraps, but are not limited thereto. The specific preparation method can be referred to as follows:
[0061] In order to remove impurities in blue leather shavings as much as possible, the blue leather shavings were added to deionized water, the pH was adjusted to 6 with a 1 mol / L aqueous solution of sodium bicarbonate, washed, filtered and dehydrated with ethanol three times. After the ethanol evaporated, it was cooled with liquid nitrogen, ground with an ultracentrifugal grinder, and passed through a 40-mesh sieve to obtain collagen fibers.
[0062] Example 1
[0063] This embodiment provides a method for preparing a collagen fiber-based foaming material, comprising the following steps:
[0064] (1) Preparation of Bayberry Tannin Modified Collagen Fibers (BT-LCF)
[0065] Dissolve 30g of bayberry tannin in 150g of deionized water and stir until it is completely dissolved to obtain a tannin solution; take 150g of collagen fiber (LCF) and place it in a reactor, add 7.5kg of deionized water, stir until the LCF is evenly dispersed in the water, add the tannin solution, adjust the pH to 5.4-5.8 with an aqueous solution of NaHCO3 with a concentration of 0.1mol / L and keep it stable, after mechanical stirring for 5h, filter through a Buchner funnel, wash the reacted solid material with anhydrous ethanol, repeat 3 times, and remove unreacted bayberry tannin; finally, dry at 80±2℃ for 24h to obtain bayberry tannin modified collagen fiber (BT-LCF).
[0066] (2) Preparation of collagen fiber-based foaming materials (WPUF / BT-LCF)
[0067] Take 30g of the BT-LCF prepared in step (1), blend it with waterborne polyurethane (WPU) in proportion (mass ratio of BT-LCF to WPU = 1:4) to obtain a mixed solution, use a high-speed stirrer to mechanically foam the mixed solution at a speed of 3000rpm, stir it at room temperature for 5min, take it out and pour it into a polytetrafluoroethylene mold, place it in an oven at 100±3℃, take it out after drying, and obtain a foamed composite material WPUF / BT-LCF.
[0068] Example 2
[0069] This embodiment refers to the preparation method of the collagen fiber-based foaming material of Embodiment 1, with the only difference being that in step (2), the mass ratio of BT-LCF to WPU is 1:9.
[0070] Example 3
[0071] This embodiment refers to the preparation method of the collagen fiber-based foaming material of Embodiment 1, with the only difference being that in step (2), the mass ratio of BT-LCF to WPU is 3:17.
[0072] Example 4
[0073] This embodiment refers to the preparation method of the collagen fiber-based foaming material of Embodiment 1, with the only difference being that in step (2), the mass ratio of BT-LCF to WPU is 1:19.
[0074] Example 5
[0075] This embodiment refers to the preparation method of the collagen fiber-based foaming material of Embodiment 1, with the only difference being that in step (2), the mass ratio of BT-LCF to WPU is 1:3.
[0076] Comparative Example 1
[0077] Comparative Example 1 refers to the preparation method of the collagen fiber-based foaming material of Example 1, except that:
[0078] The collagen fiber LCF with the same mass was used to replace the tannin modified collagen fiber BT-LCF to obtain the collagen fiber-based foaming material WPUF / LCF.
[0079] Comparative Example 2
[0080] Comparative Example 2 refers to the preparation method of the collagen fiber-based foaming material of Example 1, except that:
[0081] The same mass of opened collagen fibers DLCF was used to replace the tannin modified collagen fibers BT-LCF to obtain the collagen fiber-based foaming material WPUF / DLCF.
[0082] Among them, the opened collagen fiber DLCF is a conventional opening process of collagen fibers using mechanical equipment to break its natural multi-scale structure.
[0083] Comparative Example 3
[0084] Comparative Example 3 provides a method for preparing a collagen fiber-based foaming material, comprising the following steps:
[0085] (1) Preparation of Bayberry Tannin Modified Open Collagen Fiber (BT-DLCF)
[0086] Dissolve 30g of bayberry tannin in 150g of deionized water and stir until it is completely dissolved to obtain a tannin solution; take 150g of collagen fiber (DLCF) and place it in a reactor, add 7.5kg of deionized water, stir until DLCF is evenly dispersed in the water, add tannin solution, adjust the pH to 5.4-5.8 with an aqueous solution of NaHCO3 with a concentration of 0.1mol / L and keep it stable, after mechanical stirring for 5h, filter through a Buchner funnel, wash the reacted solid material with anhydrous ethanol, repeat 3 times to remove unreacted bayberry tannin; finally, dry at 80±2℃ for 24h to obtain bayberry tannin modified open-fiber collagen fiber (BT-DLCF).
[0087] (2) Preparation of collagen fiber-based foaming material (WPUF / BT-DLCF)
[0088] Take 30g of the BT-DLCF prepared in step (1), blend it with waterborne polyurethane (WPU) in proportion (mass ratio of BT-DLCF to WPU = 1:4) to obtain a mixed solution, use a high-speed stirrer to mechanically foam the mixed solution at a speed of 3000rpm, stir it at room temperature for 5min, take it out and pour it into a polytetrafluoroethylene mold, place it in an oven at 100±3℃, take it out after drying, and obtain a foamed composite material WPUF / BT-DLCF.
[0089] Comparative Example 4
[0090] Comparative Example 4 provides a method for preparing a foaming material, comprising the following steps:
[0091] The waterborne polyurethane (WPU) was mechanically foamed with a high-speed stirrer at a rotation speed of 3000 rpm. After stirring for 5 minutes at room temperature, it was taken out and poured into a polytetrafluoroethylene mold, placed in an oven at 100±3°C, and taken out after drying to obtain a foaming material WPUF.
[0092] Experimental Example 1
[0093] Figure 1The tensile stress-strain curves and fracture energies of WPUF / BT-LCF prepared in Example 1 of the present invention, WPUF / LCF prepared in Comparative Example 1, WPUF / DLCF prepared in Comparative Example 2, WPUF / BT-DLCF prepared in Comparative Example 3, and WPUF prepared in Comparative Example 4 are shown in FIG. The stress-strain curves of WPUF and the four composite materials are shown in FIG. Figure 1 As shown in (a), it can be seen from the figure that WPUF / BT-LCF has the highest tensile strength, which is 67% and 17% higher than WPUF and WPUF / LCF respectively. The fracture energy of WPUF and the four composite materials is shown in Figure 1 As shown in (b), among the four composite materials, WPUF / BT-LCF has the highest fracture energy, reaching 700KJ / m 3 , which is 250% higher than that of WPUF; this is because bayberry tannin can form strong hydrogen bonds with the WPUF matrix, increasing the interfacial bonding force between the fiber and the matrix, allowing stress to be transferred more effectively at the interface.
[0094] Further observation of the FESEM images of the tensile fracture surface of WPUF / BT-LCF, such as Figure 2 As shown in the figure, it can be seen that when subjected to external force, BT-LCF undergoes deflection and peeling between fibers and fiber bundles, which shows that BT-LCF has good compatibility with the WPUF matrix and has a good reinforcement effect on the WPUF matrix.
[0095] Experimental Example 2
[0096] Figure 3 The limiting oxygen index of the WPUF of the present invention and WPUF / LCF, WPUF / DLCF, WPUF / BT-LCF and WPUF / BT-DLCF with different collagen fiber contents. It can be seen from the figure that in the WPUF / BT-LCF of the present invention, due to the good compatibility of BT-LCF with the WPUF matrix and the supporting and stabilizing effect of BT-LCF on the pores in WPUF, the flame retardant performance of the composite material is significantly improved, and the limiting oxygen index is increased by 35% compared with WPUF.
[0097] In the WPUF / BT-LCF composite material of the present invention, the convective heat transfer path is increased due to the presence of pores; the collagen fibers can be evenly distributed in the WPUF substrate after modification, and since the collagen fibers themselves have a multi-level pore structure, the porosity of the foaming material is increased, thereby increasing the convective heat transfer path. When the mass fraction of BT-LCF in the composite material is 20%, the porosity of WPUF / BT-LCF is increased by 48% compared with WPUF. Figure 4The infrared thermal imaging images of the four composite materials WPUF / BT-LCF prepared in Example 1, WPUF / LCF prepared in Comparative Example 1, WPUF / DLCF prepared in Comparative Example 2, and WPUF / BT-DLCF prepared in Comparative Example 3 correspond to the surface temperature changes of the composite materials between 0 and 300 s (specifically, each composite material with a thickness of 7 mm was placed on an electric heating plate at a temperature of 100 ° C, and the WPUF / LCF, WPUF / DLCF, WPUF / B were imaged with an infrared thermal imager). T-LCF and WPUF / BT-DLCF, read and record the surface temperature every 10s, totaling 5min). It can be seen from the figure that the average temperature of the material surface at 90s is 38.6℃ (WPUF-LCF), 32.6℃ (WPUF / DLCF), 35.9℃ (WPUF / BT-LCF) and 52.8℃ (WPUF / BT-DLCF), respectively, which are 21.2℃, 16.9℃, 17.2℃ and 35.2℃ higher than the initial temperature, respectively. The temperature change scatter plot of the four WPUF composite materials from 0 to 300s is linearly fitted, and the slope obtained is the heating rate of the composite material. In summary, after LCF is modified by tannin, it can be blended with WPU to prepare foamed composite materials, which can improve their thermal insulation properties.
[0098] The present invention mainly improves the dispersibility of collagen fiber BT-LCF in the WPUF matrix by tannin modification, improves the compatibility with the WPUF matrix at the interface, is conducive to the formation of bubble cores, and plays a supporting and stabilizing role for the formed bubbles. When the mass fraction of BT-LCF in the composite material is 20%, the porosity of WPUF / BT-LCF is increased by 48% compared with WPUF, and the fracture energy is increased by 250% (reaching 700KJ / m 3 ), the limiting oxygen index increased by 35%, showing good mechanical properties, flame retardant properties and thermal insulation properties.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a collagen fiber-based foaming material, characterized in that: The steps include: foaming and molding a mixture of tannin-modified collagen fibers and waterborne polyurethane to obtain a collagen fiber-based foaming material; In the mixture, the tannin-modified collagen fiber accounts for 20 wt% to 25 wt%; The preparation of the tannin modified collagen fiber comprises: mixing tannin and collagen fiber in a liquid environment with a pH of 5.4 to 5.8, followed by washing and drying; The porosity of the collagen fiber-based foaming material is ≥50%.
2. The method for preparing the collagen fiber-based foaming material according to claim 1, characterized in that: The foaming includes any one or more combinations of mechanical foaming, physical foaming and chemical foaming.
3. The method for preparing the collagen fiber-based foaming material according to claim 2, characterized in that: The mechanical foaming method includes mechanical stirring foaming; the physical foaming method includes foaming using a physical foaming agent; and the chemical foaming method includes foaming using a chemical foaming agent.
4. The method for preparing the collagen fiber-based foaming material according to claim 3, characterized in that: In the mechanical stirring foaming, the stirring speed is 2500-3500 r / min; and the stirring time is 1-10 min.
5. The method for preparing the collagen fiber-based foaming material according to claim 3, characterized in that: The physical foaming agent includes any one or more of sodium dodecyl sulfonate, sodium dodecyl sulfate and sodium tetradecyl sulfonate.
6. The method for preparing the collagen fiber-based foaming material according to claim 3, characterized in that: The chemical foaming agent includes any one or more of azodicarbonamide, diethyl azodicarboxylate and p-toluenesulfonyl hydrazide.
7. The method for preparing the collagen fiber-based foaming material according to claim 1, characterized in that: The molding comprises: heating and drying in a mold.
8. The method for preparing the collagen fiber-based foaming material according to claim 7, characterized in that: During the molding, the drying temperature is 80-120°C.
9. The method for preparing the collagen fiber-based foaming material according to claim 1, characterized in that: The tannin-modified collagen fiber is plant tannin-modified collagen fiber; The plant tannins include any one or more mixtures of bayberry tannins, black wattle tannins, larch tannins, quebracho tannins and acacia mangium tannins.
10. The collagen fiber-based foamed material prepared by the method for preparing a collagen fiber-based foamed material according to any one of claims 1 to 9.
11. The collagen fiber-based foam material according to claim 10, characterized in that: The tensile strength of the collagen fiber-based foaming material is ≥1.2MPa, and the fracture energy is ≥650KJ / m 3 , limiting oxygen index ≥20%.
12. Use of the collagen fiber-based foam material according to claim 10 or 11 in sound insulation and heat preservation materials.
Citation Information
Patent Citations
High-cold-resistant ultrafine fiber synthetic leather used for automobiles and method of producing same
CN108103798A
Preparation method of collagen fiber-based waterborne polyurethane composite material
CN109206643A
Modified collagen fibers as well as preparation method and application thereof
CN112064346A
High-strength and toughness collagenous fiber matrix, skeleton material and structural material and preparation methods thereof
CN113463385A
Epoxidized soybean oil modified collagen fiber as well as preparation method and application thereof
CN114086390A