A SERS determination method for dibenzyl disulfide content in mineral insulating oil
Through the SERS determination method of active microcavity array substrate and nanogold substrate, the complexity and on-site detection of dibenzyl disulfide in mineral insulating oil are solved, and a rapid and accurate quantitative analysis of mg/kg order is achieved. Suitable for field applications.
Patent Information
- Application Number
- CN202211172242.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-09-26
AI Technical Summary
The prior art is difficult to quickly and accurately detect the content of dibenzyl disulfide in the order of mg/kg in mineral insulating oil, and the traditional methods are complex and require large fixed instruments, so on-site detection cannot be achieved.
Using the SERS determination method of active microcavity array substrate, the characteristic peaks are used to process the hemispherical microcavity on a quartz glass sheet, combined with the nanogold substrate and surface cleaning treatment, and combined with the CNWBONDHC-C18Cartridge solid-phase microextraction column for pre-treatment and SERS detection. The intensity is established to achieve quantitative detection of dibenzyl disulfide.
The detection process is simplified, the detection time is shortened, the detection sensitivity is improved, and it is suitable for rapid on-site inspection, avoiding the use of large fixed instruments, and achieving accurate quantities analysis of dibenzyl disulfide in mineral insulating oil.
Smart Images

Figure HDA0003863671960000011 
Figure HDA0003863671960000012 
Figure HDA0003863671960000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Raman spectroscopy analysis, and particularly relates to a SERS determination method for dibenzyl disulfide content in mineral insulating oil. Background Art
[0002] As the most basic and critical electrical equipment in the power system, the oil-immersed transformer is directly related to the safe and stable operation of the power system. Copper wires are widely used for transmission due to their excellent physical and chemical properties. In oil-immersed equipment, they are covered with multiple layers of kraft paper for insulation. The oil-paper insulation system plays a very important role in the internal insulation of the oil-immersed transformer. During the long-term operation of the transformer, the oil-paper insulation system will be affected by various factors such as mechanical stress, thermal aging and electrical aging, which will affect the performance of the transformer and even the stable operation of the power grid, causing huge material and economic losses. It is reported that many transformers in various countries around the world have failed due to sulfur corrosion in recent decades. Mineral insulating oil contains a variety of corrosive sulfides, but 90% of the corrosion problems are caused by dibenzyl disulfide. First, copper is oxidized to Cu2O in mineral insulating oil; then Cu2O reacts with the mercaptan generated by the decomposition of dibenzyl disulfide to form copper mercaptan; finally, copper mercaptan decomposes under specific conditions to form conductive Cu2S. The presence of Cu2S will cause uneven distribution of the electric field on the surface of the winding, and in severe cases, it will cause the insulation system to break down. Therefore, rapid and accurate detection of the content of dibenzyl disulfide in oil is of great significance to the safe operation of the power grid.
[0003] The content of dibenzyl disulfide in mineral insulating oil is usually in the mg / kg range. The current standard detection methods for dibenzyl disulfide are IEC62696-1:2012 issued by the International Electrotechnical Commission and GB / T32508-2016 proposed by the China Electricity Council. The former first uses gas chromatography to separate the oil sample, and then uses triple quadrupole multiple mass spectrometry (MS / MS), mass spectrometry (MS), electron capture (ECD) and atomic emission spectroscopy (AED) to detect the concentration of dibenzyl disulfide. The latter first extracts the sample with methanol, and then uses gas chromatography-mass spectrometry (GC-MS) to detect the concentration of dibenzyl disulfide. In addition to the standard method, domestic and foreign scholars have also studied other detection methods for dibenzyl disulfide in mineral insulating oil, such as combining different extraction methods with liquid chromatography (HPLC) or gas chromatography-mass spectrometry (GC-MS). In general, the detection procedure of dibenzyl disulfide is complicated and generally needs to be carried out in professional laboratories using large fixed instruments such as liquid chromatography, gas chromatography, and mass spectrometry.
[0004] As a non-destructive and efficient detection method, Raman spectroscopy has been widely used in many fields. Since the spontaneous Raman scattering signal of molecules is extremely weak, it is difficult to achieve high-sensitivity detection. With the emergence of a large number of enhanced substrates or devices, surface enhanced Raman scattering (SERS) technology has been increasingly applied to the detection of trace organic components in many actual samples, including the detection of trace components in mineral insulating oil. For example, in 2015, Japanese scholar Toshihiro Somekawa first proposed a method for directly determining the concentration of furfural in mineral insulating oil using laser Raman spectroscopy without extraction and separation. Chongqing University and other institutions have also conducted further research on the Raman spectroscopy detection of furfural in mineral insulating oil. However, the use of SERS or other Raman spectroscopy methods for quantitative detection of dibenzyl disulfide in mineral insulating oil at the mg / kg level is relatively rare. Chen Weigeng and other scholars from Chongqing University used a laboratory research-grade Raman platform to directly detect dibenzyl disulfide in insulating oil (paper DOI: 10.1109 / ICHVE.2016.7800856). The minimum detection concentration was about 150 mg / L, and the detection sensitivity was still insufficient. It is still a laboratory detection method and cannot be used for on-site detection. Patent 202110934763.3 discloses a planar structure SERS substrate with a detection limit of better than 1 mg / kg for dibenzyl disulfide in ethanol. However, it is well known in the industry that mineral insulating oil is a complex matrix composed of thousands of different compounds. The detection of components in mineral insulating oil is much more complicated than the detection of the same components in a single organic solvent. In addition, the surface of the planar structure SERS substrate used in Patent 202110934763.3 lacks a structure that can serve as a positioning mark, which increases the difficulty of accurately focusing the excitation light on the sample area in SERS detection, which is not conducive to ensuring the repeatability of the test results. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a SERS determination method for dibenzyl disulfide content in mineral insulating oil, which can simplify the Raman detection process and shorten the detection time.
[0006] In order to achieve the above object, the present invention provides the following technical solution: a SERS determination method for the content of dibenzyl disulfide in mineral insulating oil, comprising the following steps:
[0007] (1) Preparation of active microcavity array substrate:
[0008] 1.1) Processing multiple hemispherical microcavities on a quartz glass sheet, cleaning and drying the processed quartz glass sheet, and then vertically immersing it in a 0.1% mass fraction 3-aminopropyltrimethoxysilane aqueous solution, taking it out, washing it with deionized water, and drying it with nitrogen to obtain a once-immersed quartz glass sheet;
[0009] 1.2) Soak the quartz glass sheet that has been soaked once in the aqueous solution of gold nanoparticles; take it out, wash it with deionized water, blow it dry with nitrogen, put it vertically into an EP tube, add deionized water, a 0.2% chloroauric acid aqueous solution by mass fraction, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution in sequence, and immediately oscillate at an oscillation speed of 1500 rpm for 13 to 17 minutes to complete the first growth cycle, and obtain a quartz glass sheet of one growth cycle; the addition amount of 0.2% chloroauric acid aqueous solution is 140 to 160 μL per milliliter of deionized water, and the addition amount of 0.04 mol / L hydroxylamine hydrochloride aqueous solution is 70 to 80 μL;
[0010] 1.3) taking out the quartz glass sheet after one growth cycle, washing it with deionized water, blowing it dry with nitrogen, vertically placing it in an EP tube, adding deionized water, a 0.2% chloroauric acid aqueous solution, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution in sequence, wherein the amount of the 0.2% chloroauric acid aqueous solution added per milliliter of deionized water is 48 to 52 μL, and the amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution added is 24 to 26 μL, and immediately oscillating at an oscillation speed of 1500 rpm for 13 to 17 minutes to complete the second growth cycle; continuing to repeat the growth cycle according to the parameters and conditions of the second growth cycle, and after completing a total of 4 growth cycles, the active microcavity array substrate is obtained;
[0011] (2) Surface cleaning of the active microcavity array substrate: The active microcavity array substrate prepared in step 1.3) is immersed in a 0.001 mol / L potassium iodide aqueous solution for 20 min, taken out, washed with deionized water, and dried with nitrogen gas, thereby completing the surface cleaning of the active microcavity array substrate to obtain a clean SERS substrate;
[0012] (3) Pretreatment of the sample to be tested and the standard solution: The commercial CNWBONDHC-C18 Cartridge solid phase microextraction column is used to pretreat the mineral insulating oil sample to be tested and the dibenzyl disulfide / mineral insulating oil standard solutions of different concentrations; the dibenzyl disulfide / mineral insulating oil standard solutions of different concentrations contain at least 4 different concentrations of dibenzyl disulfide / mineral insulating oil standard solutions, and the dibenzyl disulfide concentration in the standard solution covers a range of 10 to 1000 mg / kg;
[0013] (4) Detection and quantification: The SERS substrate cleaned in step (2) is used to perform SERS detection on the eluate obtained by pretreatment in step (3). In the SERS spectrum of the eluate of the dibenzyl disulfide / mineral insulating oil standard solution, the dibenzyl disulfide is detected at 1006 cm -1 A calibration curve was established for the concentration of dibenzyl disulfide based on the characteristic peak intensity at 1006 cm-1 The content of dibenzyl disulfide in the sample to be tested was calculated based on the characteristic peak intensity at
[0014] Furthermore, the method for cleaning and drying the processed quartz glass sheet in step 1.1) is as follows: the processed quartz glass sheet is cleaned with aqua regia, alkali solution, and deionized water in sequence, and then dried with nitrogen.
[0015] Furthermore, in the step 1.1), the size of the quartz glass sheet is 10×20 mm, the diameter of the hemispherical microcavity is 0.8-1.2 mm, and the interval between adjacent microcavities is 2.3-2.7 mm.
[0016] Furthermore, in step 1.2), the mass fraction of the gold nanoparticle aqueous solution is 1%, and the diameter of the gold nanoparticles is 5 nm.
[0017] Furthermore, in the step 1.2), the quartz glass sheet that has been immersed once is immersed in the aqueous solution of gold nanoparticles; after being taken out and washed with deionized water and blown dry with nitrogen, it is vertically placed in an EP tube, and deionized water, a 0.2% chloroauric acid aqueous solution by mass fraction, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution are added in sequence, and the mixture is immediately oscillated at an oscillation speed of 1500 rpm for 15 to 17 minutes to complete the first growth cycle, thereby obtaining a quartz glass sheet of one growth cycle; the addition amount of the 0.2% chloroauric acid aqueous solution is 150 to 160 μL per milliliter of deionized water, and the addition amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution is 75 to 80 μL.
[0018] Furthermore, the quartz glass sheet of one growth cycle is taken out in the step 1.3), washed with deionized water, dried with nitrogen, and then placed vertically in an EP tube, and deionized water, a 0.2% chloroauric acid aqueous solution, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution are added in sequence, the amount of the 0.2% chloroauric acid aqueous solution added per milliliter of deionized water is 50-52 μL, and the amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution added is 25-26 μL, and the quartz glass sheet is immediately oscillated at an oscillation speed of 1500 rpm for 15-17 minutes to complete the second growth cycle; the growth cycle is repeated according to the parameters and conditions of the second growth cycle, and after a total of 4 growth cycles are completed, the active microcavity array substrate is obtained.
[0019] Furthermore, in the step (3), the activation solvent is first injected into the solid phase extraction column to fully wet it; then 1 mL of the mineral insulating oil sample to be tested or the dibenzyl disulfide / mineral insulating oil standard solution is fully mixed with n-hexane in a volume ratio of 1:1 to 1:3 and then added to the microextraction column, and the flow rate is controlled not to exceed 5 mL / min; after the mixed liquid has completely flowed through the column, n-hexane is added to the container containing the mixed liquid again, the container is cleaned and the cleaning liquid is also added to the microextraction column, and the flow rate is controlled not to exceed 5 mL / min; finally, the elution solvent is added to elute the dibenzyl disulfide adsorbed on the column, and the elution flow rate is controlled not to exceed 5 mL / min, and the eluate is retained for testing, thereby completing the pretreatment.
[0020] Furthermore, 1 mL of the mineral insulating oil sample or the dibenzyl disulfide / mineral insulating oil standard solution was fully mixed with n-hexane at a volume ratio of 1:2 and then added to the microextraction column.
[0021] Furthermore, the elution solvent is any one of methanol, ethanol or 3-methylpyrrolidone, and the amount of the elution solvent is 0.8 to 1.2 mL.
[0022] Furthermore, during the detection in step (4), 0.6 μL of the eluent was transferred to the microcavity of the clean SERS substrate. After the solvent evaporated naturally, the excitation light was focused to the center of the bottom of the microcavity for spectrum collection. The spectrum collection covered a range of 900-1100 cm -1 , the excitation wavelength is 532nm, 633nm or 785nm.
[0023] The SERS determination method of the dibenzyl disulfide content in mineral insulating oil of the present invention has the following beneficial effects:
[0024] 1. Compared with the existing planar structure SERS substrate with similar functions, the microcavity structure SERS enhanced substrate adopted in the present invention increases the contact area between the sample to be tested and the substrate surface, so that the sample to be tested is enriched inside the cavity, which can improve the enhancement effect; the microcavity structure SERS enhanced substrate adopted also fixes the detection area, which can simplify the Raman detection process and shorten the detection time;
[0025] 2. The surface cleaning operation process of the active microcavity array substrate used in the present invention is simple, time-saving, and has good cleaning effect, which meets the needs of rapid on-site detection;
[0026] 3. The substrate used in the present invention is a nano-gold substrate. Dibenzyl disulfide, as a sulfur-containing compound, is easy to form a sulfur-gold chemical bond with the substrate, thereby enhancing the affinity between the molecule to be tested and the surface of the substrate, making it easier for the molecule to be tested to approach the "hot spot" with a significant surface enhancement effect, thus facilitating the improvement of detection sensitivity;
[0027] 4. Compared with the national standard method for detecting dibenzyl disulfide in mineral insulating oil, the pretreatment method used in the present invention does not require mechanical oscillation and centrifugal separation, and can use organic solvents with lower toxicity. It is simple, safe, and meets the needs of rapid on-site detection;
[0028] 5. The excitation wavelength selected by the present invention is relatively close to the ultraviolet absorption of the active microcavity array substrate, which can play a good role in signal enhancement. In addition, this wavelength is convenient for selecting a portable Raman spectrometer with a small size and simple operation, avoiding the use of large fixed instruments such as liquid chromatography, gas chromatography, and mass spectrometry, and can realize on-site rapid detection of dibenzyl disulfide in mineral insulating oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The SERS spectrum of the dibenzyl disulfide standard solution eluent and the calibration curve for quantification;
[0030] Figure 2 In order to select different elution solvents for the SERS spectra of 1006 cm -1 Influence diagram of the characteristic peak intensity at ;
[0031] Figure 3 In order to select different excitation wavelengths for the SERS spectra at 1006 cm -1 Influence diagram of the characteristic peak intensity at ;
[0032] Figure 4 This is the Raman signal diagram of the same position on the active microcavity array substrate before and after cleaning. DETAILED DESCRIPTION
[0033] The following embodiments may help those skilled in the art to more fully understand the present invention, but shall not limit the present invention in any way.
[0034] Example 1
[0035] (1) Six hemispherical microcavities with a diameter of 1 mm were processed on a quartz glass sheet with a size of 10×20 mm, with an interval of 2.5 mm between adjacent microcavities. The processed quartz glass sheet was washed with aqua regia, alkali solution, and deionized water in turn, and then dried with nitrogen. It was vertically immersed in a 0.1% 3-aminopropyltrimethoxysilane aqueous solution for 20 min; taken out, washed with deionized water, dried with nitrogen, and immersed in a 5 nm diameter gold nanoparticle aqueous solution for 10 h; taken out, washed with deionized water, dried with nitrogen, and vertically placed in a 5 mL EP tube, and 2 mL of deionized water, 300 μL of 0.2% chloroauric acid aqueous solution, and 150 μL of 0.04 mol / L chloroauric acid aqueous solution were added in turn. L of hydroxylamine hydrochloride aqueous solution, immediately put the EP tube into a constant temperature mixer, oscillate at a speed of 1500rpm for 15min to complete the first growth cycle; take it out, wash it with deionized water, blow it dry with nitrogen, and vertically put it into a 5mL EP tube, add 2mL of deionized water, 100μL of 0.2% chloroauric acid aqueous solution, and 50μL of 0.04mol / L hydroxylamine hydrochloride aqueous solution in sequence, and immediately put the EP tube into a constant temperature mixer, oscillate at a speed of 1500rpm for 15min to complete the second growth cycle; continue to carry out 2 growth cycles according to the parameters and conditions of the second growth cycle, and obtain the active microcavity array substrate after completing 4 growth cycles in total.
[0036] (2) After soaking the active microcavity array substrate in a potassium iodide solution with a concentration of 0.001 mol / L for 20 minutes, the substrate was taken out and washed with deionized water and dried with nitrogen gas to complete the surface cleaning of the active microcavity array substrate.
[0037] (3) The commercial CNWBONDHC-C18 Cartridge solid phase microextraction column was used to pre-treat the mineral insulating oil samples to be tested and the dibenzyl disulfide / mineral insulating oil standard solutions with concentrations of 10 mg / kg, 50 mg / kg, 100 mg / kg, 500 mg / kg, and 1000 mg / kg, respectively. 1 mL of sample was mixed with 2 mL of n-hexane and added to the microextraction column, with the flow rate controlled not to exceed 5 mL / min. After the mixed solution completely flowed through the column, 5 mL of n-hexane was added to the container that previously contained the mixed solution, the container was cleaned and the cleaning solution was also added to the microextraction column, with the flow rate controlled not to exceed 5 mL / min. Finally, 1 mL of 3-methylpyrrolidone was added to elute the dibenzyl disulfide adsorbed on the column, with the elution flow rate controlled not to exceed 5 mL / min, and the eluate was retained for testing to complete the pre-treatment.
[0038] (4) Perform SERS detection on the eluate using the prepared active microcavity array substrate. During the detection, use a pipette to transfer 0.6 μL of the eluate into the microcavity of the active microcavity array substrate. After the solvent evaporates naturally, focus the excitation light to the center of the bottom of the microcavity for spectrum collection. The excitation wavelength is 785 nm, and the spectrum collection range is 400~1800 cm -1 In the SERS spectrum of the dibenzyl disulfide / mineral insulating oil standard solution eluent, dibenzyl disulfide is at 1006 cm -1 The characteristic peak intensity at is used to establish a calibration curve for the concentration of dibenzyl disulfide, such as Figure 1 As shown, the calibration curve equation is y=6.33x+885.79, and the determination coefficient R 2 is 0.9727, where x is the original concentration of dibenzyl disulfide in the mineral insulating oil sample, and y is the concentration of dibenzyl disulfide at 1006 cm in the SERS spectrum. -1 The characteristic peak intensity at 1006cm -1 The characteristic peak intensity at is 1731.48, and the original concentration of dibenzyl disulfide in the sample to be tested is converted to 133.6 mg / kg according to the calibration curve equation. The same sample was tested using the method in GB / T32508-2016, and the concentration of dibenzyl disulfide was 151.2 mg / kg. The relative deviation of the determination was 11.6%, which met the requirements for the reproducibility of the test results in GB / T32508-2016.
[0039] Example 2
[0040] In the pre-treatment step, the selection of different elution solvents has a great influence on the detection results. In this embodiment, methanol, ethanol, and 3-methylpyrrolidone were selected as elution solvents, and the standard solution of mineral insulating oil with a concentration of dibenzyl disulfide of 800 mg / kg was pre-treated and SERS detected. The other steps and conditions were the same as those in Example 1. The SERS spectrum at 1006 cm -1 The characteristic peak intensity at Figure 2 As shown, it can be determined that among the above three elution solvents, 3-methylpyrrolidone is the optimal elution solvent.
[0041] Example 3
[0042] In order to study the influence of the excitation wavelength on the detection results, in this embodiment, the excitation wavelengths of 532 nm, 633 nm, and 785 nm were selected respectively. The other steps and conditions were the same as those in Example 1. The standard solution of mineral insulating oil with a concentration of dibenzyl disulfide of 800 mg / kg was pretreated and SERS detected. The SERS spectra obtained under different excitation wavelengths are shown in FIG. Figure 3 As shown. According to 1006cm -1The characteristic peak intensity of dibenzyl disulfide at 785 nm can determine that among the above three excitation wavelengths, 785 nm is the optimal excitation wavelength.
[0043] Example 4
[0044] In order to study the effect of substrate surface cleaning, in this example, two substrates were prepared according to the conditions in Example 1, and the Raman signals at the same position on the substrate surface were tested before and after the substrate surface was cleaned. Figure 4 As shown in the figure, it can be observed that there are obvious impurity signals in the Raman signal of the substrate before cleaning, which causes the Raman spectrum baseline to be uneven; after surface cleaning, a flat Raman spectrum baseline is obtained. This is because iodine is easily adsorbed on the surface of the gold substrate, which is easy to replace the original impurities, and the characteristic spectrum peak formed is at 158cm -1 It does not affect the detection of the molecules to be tested, so it can produce a good cleaning effect.
[0045] From the above embodiments, it can be seen that the SERS determination method for the content of dibenzyl disulfide in mineral insulating oil provided by the present invention, compared with the existing planar structure SERS substrate with similar functions, the microcavity structure SERS enhancement substrate adopted by the present invention increases the contact area between the sample to be tested and the substrate surface, so that the sample to be tested is enriched inside the cavity, which can improve the enhancement effect; the adopted microcavity structure SERS enhancement substrate also fixes the detection area, which can simplify the Raman detection process and shorten the detection time; the surface cleaning operation process of the active microcavity array substrate adopted by the present invention is simple, time-saving, good cleaning effect, and suitable for rapid on-site detection. The invention meets the needs of detection; compared with the national standard method for detecting dibenzyl disulfide in mineral insulating oil, the pretreatment method adopted in the present invention does not require mechanical oscillation and centrifugal separation, and can select organic solvents with lower toxicity, which is simple, safe, and meets the needs of rapid on-site detection; the excitation wavelength selected by the present invention is relatively close to the ultraviolet absorption of the active microcavity array substrate, which can play a good signal enhancement role, and the wavelength is convenient for selecting a portable Raman spectrometer with small size and simple operation, avoiding the use of large fixed instruments such as liquid chromatography, gas chromatography, and mass spectrometry, and can realize rapid on-site detection of dibenzyl disulfide in mineral insulating oil.
[0046] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A SERS determination method for the content of dibenzyl disulfide in mineral insulating oil, characterized in that: The following steps are involved: (1) Preparation of active microcavity array substrate: 1.1) Processing multiple hemispherical microcavities on a quartz glass sheet, cleaning and drying the processed quartz glass sheet, and then vertically immersing it in a 0.1% mass fraction 3-aminopropyltrimethoxysilane aqueous solution, taking it out, washing it with deionized water, and drying it with nitrogen to obtain a once-immersed quartz glass sheet; 1.2) Soak the quartz glass sheet that has been soaked once in the aqueous solution of gold nanoparticles; take it out, wash it with deionized water, blow it dry with nitrogen, put it vertically into an EP tube, add deionized water, a 0.2% chloroauric acid aqueous solution by mass fraction, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution in sequence, and immediately oscillate at an oscillation speed of 1500 rpm for 13 to 17 minutes to complete the first growth cycle, and obtain a quartz glass sheet of one growth cycle; the addition amount of 0.2% chloroauric acid aqueous solution is 140 to 160 μL per milliliter of deionized water, and the addition amount of 0.04 mol / L hydroxylamine hydrochloride aqueous solution is 70 to 80 μL; 1.3) taking out the quartz glass sheet after one growth cycle, washing it with deionized water, blowing it dry with nitrogen, vertically placing it in an EP tube, adding deionized water, a 0.2% chloroauric acid aqueous solution, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution in sequence, wherein the amount of the 0.2% chloroauric acid aqueous solution added per milliliter of deionized water is 48 to 52 μL, and the amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution added is 24 to 26 μL, and immediately oscillating at an oscillation speed of 1500 rpm for 13 to 17 minutes to complete the second growth cycle; continuing to repeat the growth cycle according to the parameters and conditions of the second growth cycle, and after completing a total of 4 growth cycles, the active microcavity array substrate is obtained; (2) Surface cleaning of the active microcavity array substrate: The active microcavity array substrate prepared in step 1.3) is immersed in a 0.001 mol / L potassium iodide aqueous solution for 20 min, taken out, washed with deionized water, and dried with nitrogen gas, thereby completing the surface cleaning of the active microcavity array substrate to obtain a clean SERS substrate; (3) Pretreatment of the sample to be tested and the standard solution: The commercial CNWBONDHC-C18 Cartridge solid phase microextraction column is used to pretreat the mineral insulating oil sample to be tested and the dibenzyl disulfide / mineral insulating oil standard solutions of different concentrations; the dibenzyl disulfide / mineral insulating oil standard solutions of different concentrations contain at least 4 different concentrations of dibenzyl disulfide / mineral insulating oil standard solutions, and the dibenzyl disulfide concentration in the standard solution covers a range of 10 to 1000 mg / kg; (4) Detection and quantification: The SERS substrate cleaned in step (2) is used to perform SERS detection on the eluate obtained by pretreatment in step (3). In the SERS spectrum of the eluate of the dibenzyl disulfide / mineral insulating oil standard solution, the dibenzyl disulfide is detected at 1006 cm -1 A calibration curve was established for the concentration of dibenzyl disulfide based on the characteristic peak intensity at 1006 cm -1 The content of dibenzyl disulfide in the sample to be tested was calculated based on the characteristic peak intensity at 2. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: The method for cleaning and drying the processed quartz glass sheet in step 1.1) is as follows: the processed quartz glass sheet is cleaned with aqua regia, alkali solution, and deionized water in sequence, and then dried with nitrogen.
3. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: In the step 1.1), the size of the quartz glass sheet is 10×20 mm, the diameter of the hemispherical microcavity is 0.8-1.2 mm, and the interval between adjacent microcavities is 2.3-2.7 mm.
4. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: The mass fraction of the gold nanoparticle aqueous solution in step 1.2) is 1%, and the diameter of the gold nanoparticles is 5 nm.
5. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: In the step 1.2), the quartz glass sheet that has been immersed once is immersed in the gold nanoparticle aqueous solution; after being taken out and washed with deionized water and blown dry with nitrogen, it is vertically placed in an EP tube, and deionized water, a 0.2% chloroauric acid aqueous solution by mass fraction, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution are added in sequence, and the quartz glass sheet is immediately oscillated at an oscillation speed of 1500 rpm for 15 to 17 minutes to complete the first growth cycle, thereby obtaining a quartz glass sheet of one growth cycle; the addition amount of the 0.2% chloroauric acid aqueous solution is 150 to 160 μL per milliliter of deionized water, and the addition amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution is 75 to 80 μL.
6. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: In the step 1.3), the quartz glass sheet of one growth cycle is taken out, washed with deionized water, dried with nitrogen, and then vertically placed in an EP tube, and deionized water, a 0.2% chloroauric acid aqueous solution, and a 0.04 mol / L hydroxylamine hydrochloride aqueous solution are added in sequence, wherein the amount of the 0.2% chloroauric acid aqueous solution added is 50 to 52 μL, and the amount of the 0.04 mol / L hydroxylamine hydrochloride aqueous solution added is 25 to 26 μL per milliliter of deionized water, and the sheet is immediately oscillated at an oscillation speed of 1500 rpm for 15 to 17 minutes to complete a second growth cycle; the growth cycle is continued to be repeated according to the parameters and conditions of the second growth cycle, and after a total of 4 growth cycles are completed, the active microcavity array substrate is obtained.
7. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: In the step (3), firstly, an activation solvent is injected into the solid phase extraction column to fully wet it; then, 1 mL of the mineral insulating oil sample to be tested or the dibenzyl disulfide / mineral insulating oil standard solution is fully mixed with n-hexane in a volume ratio of 1:1 to 1:3 and then added to the microextraction column, and the flow rate is controlled not to exceed 5 mL / min; after the mixed liquid completely flows through the column, n-hexane is added to the container containing the mixed liquid again, the container is cleaned and the cleaning liquid is also added to the microextraction column, and the flow rate is controlled not to exceed 5 mL / min; finally, an elution solvent is added to elute the dibenzyl disulfide adsorbed on the column, and the elution flow rate is controlled not to exceed 5 mL / min, and the eluate is retained for testing, thereby completing the pretreatment.
8. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 7, characterized in that: 1 mL of the mineral insulating oil sample or dibenzyl disulfide / mineral insulating oil standard solution was fully mixed with n-hexane in a volume ratio of 1:2 and then added to the microextraction column.
9. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 7, characterized in that: The elution solvent is any one of methanol, ethanol or 3-methylpyrrolidone, and the amount of the elution solvent is 0.8 to 1.2 mL.
10. The SERS determination method for dibenzyl disulfide content in mineral insulating oil according to claim 1, characterized in that: During the detection in step (4), 0.6 μL of the eluent is transferred to the microcavity of the clean SERS substrate. After the solvent evaporates naturally, the excitation light is focused to the center of the bottom of the microcavity for spectrum collection. The spectrum coverage range is 900-1100 cm -1 , the excitation wavelength is 532nm, 633nm or 785nm.
Citation Information
Patent Citations
Preparation method of surface plasmonic crystal
CN101698961A
Reversed phase high performance liquid chromatography method for determining content of dibenzyl disulfide in insulating oil
CN105974042A
Preparation method of surface-enhanced raman substrate of zinc oxide-silver composite microcavity structure
CN107356584A
Method for measuring content of benzotriazole in transformer oil
CN113533303A
Preparation method of solid-phase SERS nano-substrate
CN113588625A