A film forming method for improving warpage

By injecting air from the bottom of the furnace cavity in the low-pressure chemical vapor deposition furnace and adjusting the length and position of the air inlet pipe to control the reaction gas concentration, the problem of silicon wafer warping caused by the gradient in the temperature zone of the vertical furnace was solved and more uniform film formation was achieved process and improve product yield.

CN115613007BActive Publication Date: 2024-10-01SHANGHAI SEMICON WAFER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211251913.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2024-10-01
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

In the vertical low-pressure chemical vapor deposition furnace, the large temperature gradient causes the silicon wafer to warp significantly, affecting the yield of the product wafer.

Method used

By injecting air from the bottom of the furnace cavity in a low-pressure chemical vapor deposition furnace, adjusting the length and position of the air inlet pipe, controlling the concentration of reaction gases, and reducing the temperature difference between temperature zones, thereby reducing warpage.

Benefits of technology

It effectively reduces the warpage change rate of silicon wafers and improves the uniformity of the film forming process and the product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115613007B_ABST
    Figure CN115613007B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology. A film forming method for improving warpage, characterized in that, when a film forming process is performed by a low-pressure chemical vapor deposition furnace, an air inlet pipe takes in air from the bottom of the furnace chamber, and the warpage of the silicon wafer after the film forming process is adjusted by adjusting the length of the air inlet pipe extending into the furnace chamber of the low-pressure chemical vapor deposition furnace. Since the concentration of the reaction gas at the bottom is relatively high, it decreases in steps to the top. The present application extends the air inlet pipe into the furnace, so that the concentration in the middle is higher and decreases in steps toward the two ends, the difference between the temperature zones becomes smaller, and the warpage change also becomes smaller. The concentration of the reaction gas in each temperature zone in the furnace is changed by changing the position of the air inlet pipe, thereby affecting the temperature of each temperature zone in the furnace, and further improving the warpage at some positions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a film forming method. Background Art

[0002] At present, the vertical low-pressure chemical vapor deposition technology is the main deposition method for polysilicon back seal. Due to the vertical furnace body, the warpage caused by various parts in the furnace varies greatly, and some positions are prone to cause excessive warpage of silicon wafers and result in yield loss.

[0003] There are four temperature zones with different temperatures from top to bottom in the vertical low-pressure chemical vapor deposition furnace, and from bottom to top in the vertical low-pressure chemical vapor deposition furnace there are the M7 layer, M6 layer, M5 layer, M4 layer, M3 layer, M2 layer and M1 layer for placing silicon wafers.

[0004] After testing, the warpage change at the M7 position is significantly larger than that at the M1 position. The main reasons for the adverse warpage changes in various parts of the furnace are: the reaction chamber is a vertical, single-tube bottom air intake structure; it can meet customers' requirements for film thickness and uniformity within the product sheet, but because the gradient between the four temperature zones is relatively large: the lower the temperature, the lower the temperature, and after single-side polishing, the warp increases significantly (the increase in warpage also shows a gradient increase pattern, the greater the increase in warpage is, the closer to the BOTTOM end).

[0005] Currently, there is a lack of a film forming method that can achieve warpage control in a vertical low-pressure chemical vapor deposition furnace. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides a film forming method with improved warping to solve at least one of the above technical problems.

[0007] In order to achieve the above-mentioned purpose, the present invention provides a film forming method with improved warping, which is characterized in that when the film forming process is carried out through a low-pressure chemical vapor deposition furnace, an air inlet pipe takes in air from the bottom of the furnace chamber, and the warping rate of the silicon wafer after the film forming process is adjusted by adjusting the length of the air inlet pipe extending into the furnace chamber of the low-pressure chemical vapor deposition furnace.

[0008] Further preferably, there are seven silicon wafer placement layers from top to bottom in the furnace chamber;

[0009] The top of the air inlet pipe is located between the third silicon wafer arrangement layer and the seventh silicon wafer arrangement layer from top to bottom.

[0010] Further preferably, the air inlet pipe is a telescopic pipe, so that the length can be adjusted according to the requirements.

[0011] Further preferably, the air inlet pipe includes a vertical portion which is vertically arranged and located in the furnace cavity;

[0012] The side wall of the vertical portion is provided with air outlet holes, and the apertures of the air outlet holes increase from top to bottom.

[0013] Further preferably, the air inlet pipe is a pipe made of quartz material.

[0014] Further preferably, when the deposition thickness of the film forming process is 300-1000 nm, the film forming process comprises the following steps:

[0015] Step 1, cleaning the single crystal silicon wafer;

[0016] Step 2: Place the cleaned single crystal silicon wafer on a silicon boat made of SiC for heat treatment. The principle is to deposit pure single crystal silicon on the back of the silicon wafer through the thermal decomposition of SiH4. The heat treatment method of the single crystal silicon wafer is as follows: before heating, place the cleaned single crystal silicon wafer on the silicon boat and introduce high-purity nitrogen into the furnace for 15 to 25 minutes to drive out the gas. Then, slowly heat the silicon boat to 500 to 700°C and keep it for 20 to 60 minutes. Then, slowly cool it down and take out the single crystal silicon wafer. At this time, a layer of polycrystalline silicon film is formed on the surface of the single crystal silicon.

[0017] In step 2, during the thermal decomposition process, chemical vapor deposition is used to deposit a polycrystalline silicon film on the single crystal silicon wafer after thermal oxidation treatment using silane as the reaction gas. The process parameters for depositing the polycrystalline silicon film on the single crystal silicon wafer after thermal oxidation treatment are: RF power 100-150W, RF frequency 13.56MHz, substrate temperature 500-700℃, chamber pressure 20-35Pa, SiH4 gas with a purity of 99.999% by volume 0.8-1.2slm, and deposition time 20-60 minutes.

[0018] Further preferably, during the film forming process, when the air flow rate of the air inlet pipe is controlled at 0.8-1.2slm, SiH4 gas is input for 20 to 60 minutes, and the temperature in the furnace chamber is controlled in four temperature zones of 640±50°C from top to bottom.

[0019] There are four temperature zones from top to bottom in the furnace cavity, namely the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone;

[0020] When the air inlet pipe input height is 15 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 640°C and 638°C respectively, and the reaction time is 20-60min;

[0021] When the air inlet pipe input height is 35 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 645°C and 647°C respectively, and the reaction time is 20-60 min;

[0022] When the air inlet pipe input height is 57 cm from the furnace mouth, the reaction gas SiH4 is input, the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 640°C, 642°C, 648°C and 651°C respectively, and the reaction time is 20-60min.

[0023] By changing the different heights of the air inlet pipe in the furnace chamber, the concentrations at different positions in the furnace chamber tend to be consistent, thereby reducing the temperature difference at different positions in the furnace chamber and reducing the amount of warpage change.

[0024] Further preferably, after film formation, the warpage change rate of the silicon wafer is controlled within WARPBF≤15.

[0025] Beneficial effects:

[0026] Since the concentration of the reaction gas at the bottom is relatively high, it decreases in steps to the top. In this application, the inlet pipe is extended into the furnace, so that the concentration in the middle is relatively high and decreases in steps to both ends, the difference between the temperature zones becomes smaller, and the warpage change amount also becomes smaller.

[0027] By changing the position of the air inlet pipe, the concentration of the reaction gas in each temperature zone in the furnace was changed, thereby affecting the temperature of each temperature zone in the furnace and further improving the warping at some locations. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a structural schematic diagram of a specific embodiment 1 of the present invention.

[0029] Among them: 1 is the intake pipe. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the accompanying drawings.

[0031] See also Figure 1 , Specific embodiment 1, a film forming method for improving warpage, characterized in that, when the film forming process is carried out through a low-pressure chemical vapor deposition furnace, an air inlet pipe takes in air from the bottom of the furnace chamber, and the warpage rate of the silicon wafer after the film forming process is adjusted by adjusting the length of the air inlet pipe extending into the furnace chamber of the low-pressure chemical vapor deposition furnace.

[0032] There are seven silicon wafer layers from top to bottom in the furnace chamber; the top of the air inlet pipe is located between the third silicon wafer layer and the seventh silicon wafer layer from top to bottom. The seven silicon wafer layers are the first silicon wafer layer, the second silicon wafer layer, the third silicon wafer layer, the fourth silicon wafer layer, the fifth silicon wafer layer, the sixth silicon wafer layer and the seventh silicon wafer layer from top to bottom.

[0033] The air inlet pipe 1 is a telescopic pipe, which is convenient for adjusting the length according to needs.

[0034] The air inlet pipe 1 comprises a vertical portion which is vertically arranged and located in the furnace cavity; a side wall of the vertical portion is provided with air outlet holes, and the apertures of the air outlet holes increase from top to bottom.

[0035] The air intake pipe is made of quartz.

[0036] When the deposition thickness of the film forming process is 300-1000nm, the film forming process includes the following steps:

[0037] Step 1, cleaning the single crystal silicon wafer;

[0038] Step 2: Place the cleaned single crystal silicon wafer on a silicon boat made of SiC for heat treatment. The principle is to deposit pure single crystal silicon on the back of the silicon wafer through the thermal decomposition of SiH4. The heat treatment method of the single crystal silicon wafer is as follows: before heating, place the cleaned single crystal silicon wafer on the silicon boat and introduce high-purity nitrogen into the furnace for 15 to 25 minutes to drive out the gas. Then, slowly heat the silicon boat to 500 to 700°C and keep it for 20 to 60 minutes. Then, slowly cool it down and take out the single crystal silicon wafer. At this time, a layer of polycrystalline silicon film is formed on the surface of the single crystal silicon.

[0039] In step 2, during the thermal decomposition process, chemical vapor deposition is used to deposit a polycrystalline silicon film on the single crystal silicon wafer after thermal oxidation treatment using silane as the reaction gas. The process parameters for depositing the polycrystalline silicon film on the single crystal silicon wafer after thermal oxidation treatment are: RF power 100-150W, RF frequency 13.56MHz, substrate temperature 500-700℃, chamber pressure 20-35Pa, SiH4 gas with a purity of 99.999% by volume 0.8-1.2slm, and deposition time 20-60 minutes.

[0040] Specific embodiment 2, based on specific embodiment 1, during the film forming process, when the air flow rate of the air inlet pipe is controlled at 0.8-1.2slm, SiH4 gas is input, the time is controlled at 20-60 minutes, and the temperature in the furnace chamber is controlled in four temperature zones of 640±50℃ from top to bottom.

[0041] There are four temperature zones from top to bottom in the furnace cavity, namely the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone;

[0042] When the air inlet pipe is 15 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 640°C and 638°C respectively, and the reaction time is 20-60 minutes. At this time, the top of the air inlet pipe is at the seventh silicon wafer placement layer.

[0043] When the air inlet pipe is 35 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 645°C and 647°C respectively, and the reaction time is 20-60 minutes. At this time, the top of the air inlet pipe is at the fifth silicon wafer placement layer.

[0044] When the air inlet pipe is 57 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 640°C, 642°C, 648°C and 651°C respectively, and the reaction time is 20-60 minutes. At this time, the top of the air inlet pipe is at the third silicon wafer placement layer.

[0045] By changing the different heights of the air inlet pipe in the furnace chamber, the concentrations at different positions in the furnace chamber tend to be consistent, thereby reducing the temperature difference at different positions in the furnace chamber and reducing the amount of warpage change.

[0046] The distance from the furnace mouth is the bottom position of the vertical part.

[0047]

[0048] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A film forming method for improving warpage, characterized in that: When the film forming process is carried out through the low-pressure chemical vapor deposition furnace, the air inlet pipe takes in air from the bottom of the furnace chamber, and the warpage of the silicon wafer after the film forming process is adjusted by adjusting the length of the air inlet pipe extending into the furnace chamber of the low-pressure chemical vapor deposition furnace; When the deposition thickness of the film forming process is 300-1000nm, the film forming process includes the following steps: Step 1, cleaning the single crystal silicon wafer; Step 2: Place the cleaned single crystal silicon wafer on a silicon boat made of SiC material for thermal processing. The principle is to deposit pure single crystal silicon on the back of the silicon wafer through the thermal decomposition of SiH4. The heat treatment method of the single crystal silicon wafer is as follows: before heating, place the cleaned single crystal silicon wafer on the silicon boat and introduce nitrogen into the furnace for 15 to 25 minutes to drive out the gas. Then, slowly heat the silicon boat to 500 to 700°C and keep it for 20 to 60 minutes. Then, slowly cool it down and take out the single crystal silicon wafer. At this time, a layer of polysilicon film is formed on the surface of the single crystal silicon. In step 2, during the thermal decomposition process, a polycrystalline silicon film is deposited on the single-crystalline silicon wafer after thermal oxidation by chemical vapor deposition using silane as the reaction gas. The process parameters for depositing the polycrystalline silicon film on the single-crystalline silicon wafer after thermal oxidation are: RF power 100-150W, RF frequency 13.56MHz, substrate temperature 500-700°C, chamber pressure 20-35Pa, SiH4 gas flow rate of 99.999% by volume, 0.8-1.2slm, and deposition time 20-60 minutes; During the film forming process, when the air flow rate of the air inlet pipe is controlled at 0.8-1.2slm, SiH4 gas is input for 20-60 minutes, and the temperature in the furnace chamber is controlled in four temperature zones of 640±50℃ from top to bottom; There are four temperature zones from top to bottom in the furnace cavity, namely the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone; When the air inlet pipe input height is 15 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 640°C and 638°C respectively, and the reaction time is 20-60min; When the air inlet pipe input height is 35 cm from the furnace mouth, the reaction gas SiH4 is input, and the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 650°C, 646°C, 645°C and 647°C respectively, and the reaction time is 20-60 min; When the air inlet pipe input height is 57 cm from the furnace mouth, the reaction gas SiH4 is input, the temperatures of the first temperature zone, the second temperature zone, the third temperature zone and the fourth temperature zone are 640°C, 642°C, 648°C and 651°C respectively, and the reaction time is 20-60min.

2. A film forming method for improving warpage according to claim 1, characterized in that: The air inlet pipe includes a vertical portion which is vertically arranged and located in the furnace cavity; The side wall of the vertical portion is provided with air outlet holes, and the apertures of the air outlet holes increase from top to bottom.

3. A film forming method for improving warpage according to claim 1, characterized in that: The air inlet pipe is a pipe made of quartz.