A method for chemical bath deposition of mesoporous tin dioxide thin film
The mesoporous tin dioxide film was prepared by low-temperature chemical bath deposition, which solved the problems of complex operation, high energy consumption and poor particle dispersion in the prior art, and realized a mesoporous tin dioxide film with controllable thickness and excellent material performance. It is applied to perovskite solar cells to obtain high-efficiency photoelectric conversion effect.
Patent Information
- Application Number
- CN202210185526.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The existing chemical bath deposition method has problems such as complex operation, high energy consumption, high cost and poor particle dispersion. It is difficult to accurately control the thickness of dense tin dioxide, and it is easy to produce pinholes or micro holes, which affects the performance of the material.
Low-temperature chemical bath deposition method is used to form a transparent homogeneous solution by adding urea, concentrated hydrochloric acid, thioglycolic acid and tin source to water, aged at room temperature and deposited in situ on the surface of the substrate, and the reaction time is controlled to prepare a thickness of 60-200nm. Mesoporous tin dioxide film uses stannous chloride as the tin source and water as the reaction solvent to regulate the thickness and structure of tin dioxide by controlling the reaction time and temperature.
It realizes the preparation of mesoporous tin dioxide films with low cost and simple process, excellent material performance, is used in the electron transport layer of perovskite solar cells, and obtains a photoelectric conversion efficiency of 24.11%, controllable thickness, uniform particle distribution, and simple operation .
Smart Images

Figure CN115637426B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials, and in particular relates to a method for chemical bath deposition of a mesoporous tin dioxide film. Background Art
[0002] Tin dioxide is a wide-bandgap metal semiconductor material with an electron mobility of ~240 cm 2 V -1 S -1 , optical band gap is 3.6-4.0eV, high transmittance, chemical stability, mechanical stability and other advantages, and is widely used in photovoltaic devices, touch screens, flat panel displays, energy-saving smart windows and other fields. Therefore, the synthesis of tin dioxide is of great significance.
[0003] At present, the synthesis methods of tin dioxide mainly include sol-gel method, hydrothermal synthesis, chemical bath deposition, atomic layer deposition and spray deposition. Among them, for the traditional chemical bath deposition method, it is generally necessary to be in a high temperature environment, and dense tin dioxide is obtained. However, if the thickness of dense tin dioxide cannot be accurately controlled, pinholes or microholes are easily generated, thereby affecting the performance of tin dioxide, and in order to eliminate this adverse effect, an effective method for preparing tin dioxide needs to be provided. Summary of the invention
[0004] The invention aims to solve the problems of complex operation, high energy consumption, high cost and poor particle dispersibility in the prior art, and provides a method for preparing a mesoporous tin dioxide film by chemical bath.
[0005] To achieve the above purpose, the present invention adopts the following technical solution:
[0006] A method for chemical bath deposition of a mesoporous tin dioxide film comprises adding urea, concentrated hydrochloric acid, thioglycolic acid and a tin source into water to obtain a transparent homogeneous solution, aging the obtained transparent homogeneous solution at low temperature, and then immersing a substrate in the aged transparent homogeneous solution to in-situ deposit a mesoporous tin dioxide film with a thickness of 60-200 nm on the surface of the substrate at low temperature.
[0007] Furthermore, urea, concentrated hydrochloric acid, thioglycolic acid and a tin source are added to water to obtain a transparent homogeneous solution, and the obtained transparent homogeneous solution is aged at room temperature for 2-20 days (generally 2-4 days), and then the substrate is immersed in the aged transparent homogeneous solution and in situ deposited on the surface of the substrate at room temperature for 2-4 days, so that a mesoporous tin dioxide film with a thickness of 60-200 nm is formed on the surface of the substrate.
[0008] Going further,
[0009] (1) preparing a solution required for chemical bath deposition, and sequentially adding urea, concentrated hydrochloric acid, thioglycolic acid, and a tin source into the aqueous solution to form a transparent homogeneous solution;
[0010] (2) leaving the transparent homogeneous solution at room temperature for more than 2 days;
[0011] (3) placing a glass (the other side of the glass can be taped with nylon tape to prevent material deposition) vertically into the transparent homogeneous solution prepared in step (2) and subjecting it to a chemical bath reaction at room temperature for 2-4 days;
[0012] (4) After the reaction is completed, the glass is taken out and cleaned to obtain a mesoporous tin dioxide film.
[0013] After the reaction, the substrate is taken out for cleaning and annealing, so that a mesoporous tin dioxide film is obtained on the surface of the substrate.
[0014] The annealing temperature is 150-170° C., and the reaction time is 0.5-2 h.
[0015] The final concentration of urea in the transparent homogeneous solution is 0.02-0.2 mol / L, and the final concentration of the tin source is 0.002-0.012 mol / L;
[0016] In the transparent homogeneous solution, the volume ratio of water to concentrated hydrochloric acid is 100:0.5-100:1.25, and the volume ratio of water to thioglycolic acid is 10000:0.5-10000:2.5.
[0017] The concentration of the concentrated hydrochloric acid is 0.03-0.15 mol / L; the concentration of the thioglycolic acid is 0.5-2.75 mmol / L.
[0018] The tin source is stannous chloride and / or stannous chloride dihydrate.
[0019] A mesoporous tin dioxide film is prepared by the method described above. The mesoporous tin dioxide film with a thickness of 60-200 nm is obtained by the method described above.
[0020] An application of a mesoporous tin dioxide film, and an application of the mesoporous tin dioxide film in an electron transport layer material for a perovskite solar cell.
[0021] The working principle of the present invention:
[0022] The present invention adopts stannous chloride as a tin source and water as a reaction solvent, and can obtain a mesoporous tin dioxide film on a conductive glass, and can obtain a mesoporous tin dioxide film of different thicknesses by controlling the reaction time. Under low temperature conditions, the tin dioxide deposited by a chemical bath is in a mesoporous state because, under low temperature conditions, thioglycolic acid as a structural linker will degrade, so that the state of the solvent changes, the solvent shell rearranges, the tin dioxide particles grow, and are interconnected through organic chains to form mesoporous tin dioxide.
[0023] The advantages of the present invention are:
[0024] The present invention changes the temperature of chemical bath deposition and solution aging time during the preparation of tin oxide thin film, controls the deposition time, and grows a layer of mesoporous tin dioxide thin film on a substrate; the material cost adopted in the present invention is low, the process is simple, and the preparation is carried out at low temperature, thereby realizing a method for preparing mesoporous tin dioxide thin film at low cost; the formed mesoporous tin dioxide can be further applied in perovskite solar cells; specifically:
[0025] (1) Simple operation: The present invention adopts a simple chemical bath deposition method to obtain a mesoporous tin dioxide film assembled by nanoparticles in one step, and the process is simple.
[0026] (2) Controllable thickness: The present invention can obtain mesoporous tin dioxide of different thicknesses by adjusting the reaction time.
[0027] (3) Homogeneous distribution: The chemical bath reaction liquid used in the present invention has uniform distribution of tin dioxide particles.
[0028] (4) Excellent product performance: The tin dioxide film deposited in the present invention has excellent photoelectric performance and can achieve a photoelectric conversion efficiency of 24.11% when used in an organic-inorganic hybrid perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The X-ray diffraction (XRD) spectrum of the tin dioxide powder prepared in Example 1 of the present invention;
[0030] Figure 2 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 1 day in Example 2 of the present invention;
[0031] Figure 3 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 2 days in Example 2 of the present invention;
[0032] Figure 4 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 3 days in Example 2 of the present invention;
[0033] Figure 5 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 4 days in Example 2 of the present invention;
[0034] Figure 6 The X-ray diffraction (XRD) spectrum of tin dioxide prepared in Example 3 of the present invention;
[0035] Figure 7 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 1 day in Example 4 of the present invention;
[0036] Figure 8 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 2 days in Example 4 of the present invention;
[0037] Fig. 9 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 3 days in Example 4 of the present invention;
[0038] Fig.10 The scanning electron microscope (SEM) photos of the plane and cross section of the tin dioxide film deposited for 4 days in Example 4 of the present invention;
[0039] Fig.11 The nanoparticle size distribution diagram of the tin dioxide solution prepared in Example 5 of the present invention, (a) is the nanoparticle size distribution diagram of the upper solution, and (b) is the nanoparticle size distribution diagram of the lower solution;
[0040] Fig.12 The nanoparticle size distribution diagram of the tin dioxide solution prepared in Example 6 of the present invention, (a) is the nanoparticle size distribution diagram of the upper solution, and (b) is the nanoparticle size distribution diagram of the lower solution;
[0041] Fig.13 This is the JV curve of the perovskite solar cell prepared in the application example of the present invention.
[0042] Fig.14 Distribution of photoelectric conversion efficiency of perovskite solar cells prepared with planar and mesoporous SnO2 layers. DETAILED DESCRIPTION
[0043] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.
[0044] Example 1
[0045] Weigh 3.125g of urea, add 250mL of water, wait until the urea is completely dissolved, then add 3.125mL of hydrochloric acid, 62.5uL of thioglycolic acid and 687.5mg of dihydrated tin dichloride to the solution in sequence. After the solute is completely dissolved, the solution is placed at room temperature for two days. Then, a glass slide is placed vertically in the solution. After four days of reaction, the material on the glass slide is scraped off with a blade to obtain a powder for material analysis (see Figure 1 ).
[0046] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0047] Figure 1 : is the X-ray diffraction (XRD) spectrum of the obtained powder. From the spectrum, it can be known that since the peak position is consistent with that described in standard PDF#41-1445, tin dioxide can be generated at room temperature without annealing treatment.
[0048] Example 2
[0049] Weigh 3.125g urea, add 250mL water, wait until the urea is completely dissolved, then add 3.125mL hydrochloric acid, 62.5uL thioglycolic acid and 687.5mg tin dichloride dihydrate to the solution in sequence. After the solute is completely dissolved, leave it at room temperature for two days, then place the conductive glass (stick the glass surface that does not need to be deposited with nylon tape) vertically into the solution. Leave the solution to deposit at room temperature for 1-4 days, and obtain tin dioxide films with different deposition times and different deposition thicknesses (see Figure 2-4 ).
[0050] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0051] Figure 2 This is the SEM image of the tin dioxide film obtained after one day of deposition. Figure 3 This is the SEM image of the tin dioxide film obtained after 2 days of deposition. Figure 4 This is the SEM image of the tin dioxide film obtained after 3 days of deposition. Figure 5 The SEM images of the tin dioxide film obtained after 4 days of deposition are obtained from different deposition times. When the deposition time is one day, there is no substance on the conductive glass; when the deposition time is two days, the conductive glass is covered with a layer of mesoporous tin dioxide with a thickness of 60nm; when the deposition time is three days, the conductive glass is covered with a layer of mesoporous tin dioxide with a thickness of 140nm; when the deposition time is four days, the conductive glass is covered with a layer of mesoporous tin dioxide with a thickness of 200nm.
[0052] Example 3
[0053] Weigh 3.125g of urea, add 250mL of water, wait until the urea is completely dissolved, then add 3.125mL of hydrochloric acid, 62.5uL of thioglycolic acid and 687.5mg of dihydrated tin dichloride to the solution in sequence. After the solute is completely dissolved, leave the solution at room temperature for two days. Then place a glass piece vertically in the solution and place it together in an oven at 70°C. After four days of reaction, scrape the material on the glass piece with a blade and obtain a powder for material analysis (see Figure 6 ).
[0054] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0055] Figure 6 : is the X-ray diffraction (XRD) spectrum of the obtained powder. From the spectrum, it can be known that since the peak position is consistent with that described in standard PDF#41-1445, when the chemical bath reaction temperature is 70°C, tin dioxide can be generated even without annealing treatment.
[0056] Example 4
[0057] Weigh 3.125g urea, add 250mL water, wait until the urea is completely dissolved, then add 3.125mL hydrochloric acid, 62.5uL thioglycolic acid and 687.5mg tin dichloride dihydrate to the solution in sequence. When the solute is completely dissolved, leave it at room temperature for two days. Then put the conductive glass (stick the glass surface that does not need to be deposited with nylon tape) vertically into the solution. Deposit the solution in an oven at 70°C for 1-4 days to obtain tin dioxide films with different deposition times and different deposition thicknesses (see Figure 7-10 )
[0058] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0059] Figure 7 This is the SEM image of the tin dioxide film obtained after one day of deposition. Figure 8 This is the SEM image of the tin dioxide film obtained after 2 days of deposition. Fig. 9 This is the SEM image of the tin dioxide film obtained after 3 days of deposition. Fig.10 This is a SEM image of the tin dioxide film obtained after 4 days of deposition. Figure 7-10 It can be seen that the deposited tin dioxide is a dense planar tin dioxide film with thicknesses of 230nm, 430nm, 570nm and 650nm, respectively.
[0060] Example 5
[0061] Weigh 3.125g urea, add 250mL water, wait until the urea is completely dissolved, then add 3.125mL hydrochloric acid, 62.5uL thioglycolic acid and 687.5mg tin dichloride dihydrate to the solution. When the solute is completely dissolved, place the solution at room temperature for 3 days. Use a pipette to take the upper and lower solutions respectively and place them in a small bottle.
[0062] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0063] Fig.11 The graph shows the particle size distribution of nanoparticles in the prepared tin dioxide solution. (a) is the particle size distribution of nanoparticles in the upper solution, and (b) is the particle size distribution of nanoparticles in the lower solution. It can be seen from the graph that the particle size distribution of nanoparticles in the upper and lower solutions is relatively uniform, mainly because the reaction conditions are relatively mild, the particle formation and growth rate is slow, and the particle distribution is relatively uniform.
[0064] Example 6
[0065] Weigh 3.125g urea, add 250mL water, wait until the urea is completely dissolved, then add 3.125mL hydrochloric acid, 62.5uL thioglycolic acid and 687.5mg tin dichloride dihydrate to the solution. When the solute is completely dissolved, place the solution at room temperature for 2 days, then place the solution in an oven at 70℃ for 1 day. Use a pipette to take the upper and lower solutions respectively and place them in a vial.
[0066] The concentration of the above concentrated hydrochloric acid is 0.15 mol / L; the concentration of thioglycolic acid is 2.75 mmol / L.
[0067] Fig.12 The graph shows the particle size distribution of nanoparticles in the prepared tin dioxide solution. (a) is the particle size distribution of nanoparticles in the upper solution, and (b) is the particle size distribution of nanoparticles in the lower solution. It can be seen from the graph that the particle size distribution of nanoparticles in the upper and lower solutions is uneven, and the particles are seriously deposited, resulting in larger particles in the lower solution.
[0068] Application Examples
[0069] First, a mesoporous tin dioxide film was deposited for 3 days by using Example 2 to obtain a completely covered mesoporous tin dioxide electron transport layer.
[0070] Secondly, 1.53M PbI2, 1.4M FAI, 0.5M MACl and 0.122M MAPbBr3 were added to a mixed solvent of DMF:DMSO=8:1 (v / v) to prepare a perovskite precursor solution. The prepared precursor solution was used to prepare a perovskite film by a one-step method. The specific steps were as follows: 35uL of the precursor solution was dropped on the prepared tin dioxide films with different thicknesses using a pipette. After the liquid was spread, 1000rpm for 10s; 4000rpm for 30s. Finally, 350uL of anisole was added to the film for 25s to obtain an unannealed wet perovskite film. The obtained perovskite film was then placed on a hot plate at 100°C for annealing.
[0071] Then, weigh 50 mg of Spiro-OMeTAD powder, add 19.5 μL of tBP, 5 μL of Co(Ⅲ)TFSI solution (0.25 M in acetonitrile), 5 μL of Li-TFSI solution (0.25 M in acetonitrile) and 1 mL of chlorobenzene in turn, stir thoroughly and use. Take 35 uL of the solution and drop it on the above annealed perovskite film, and spin coat at 3000 r for 30 s.
[0072] Finally, 60nm of gold was evaporated on the prepared film as an electrode to prepare a perovskite solar cell device.
[0073] The JV curve of the perovskite solar cell was tested by the Newport Oriel test system under a standard solar light source (the instrument parameters were set to AM 1.5 and the light intensity was 100 MW / cm 2 ), and the open circuit voltage (V OC ), short-circuit current density (J SC ), fill factor (FF) and photoelectric conversion efficiency (PCE) and other important parameters. Fig.13 is the JV curve of the prepared perovskite solar cell, where V OC =1.18V, J SC =25.17mA·cm -2 , FF=81.18%, PCE=24.11%.
[0074] At the same time, the performance of the obtained mesoporous tin dioxide film was further tested:
[0075] The mesoporous tin dioxide film deposited for 3 days in Example 2 was used to obtain a completely covered mesoporous tin dioxide electron transport layer; 20 perovskite solar cells with the mesoporous tin dioxide film as the electron transport layer were assembled according to the steps of the perovskite solar cell device described above, and were set aside;
[0076] In addition, a planar tin dioxide film was obtained in the manner described in Example 4, wherein the deposition reaction temperature was 70° C. and the deposition was carried out in an oven for 2 h to obtain a planar tin dioxide film as a control group, and then 20 perovskite solar cells with a planar tin dioxide film as an electron transport layer were assembled according to the steps of the perovskite solar cell device described above, and then used for standby;
[0077] The perovskite solar cell obtained above was subjected to JV curve test according to the existing method (see Fig.14 ).
[0078] As can be seen from the figure, the photoelectric conversion efficiency of perovskite solar cells prepared with mesoporous tin dioxide layers is higher than that of planar tin dioxide layers, so the mesoporous layer has more advantages than the planar layer.
Claims
1. A method for chemical bath deposition of mesoporous tin dioxide thin films, Features: Adding urea, concentrated hydrochloric acid, thioglycolic acid and a tin source to water to obtain a transparent homogeneous solution, aging the obtained transparent homogeneous solution at room temperature for 2-20 days, and then immersing a substrate in the aged transparent homogeneous solution, and in-situ depositing on the surface of the substrate at room temperature for 2-4 days, i.e. forming a mesoporous tin dioxide film with a thickness of 60-200 nm on the surface of the substrate; The final concentration of urea in the transparent homogeneous solution is 0.02-0.2 mol / L, and the final concentration of the tin source is 0.002-0.012 mol / L; In the transparent homogeneous solution, the volume ratio of water to concentrated hydrochloric acid is 100:0.25-100:1.25, and the volume ratio of water to thioglycolic acid is 10000:0.5-10000:2.
5.
2. The method for preparing mesoporous tin dioxide by chemical bath according to claim 1, Features: After the reaction, the substrate is taken out for cleaning and annealing, so that a mesoporous tin dioxide film is obtained on the surface of the substrate.
3. The method for preparing mesoporous tin dioxide by chemical bath according to claim 2, Features: The annealing temperature is 150-170° C., and the reaction time is 0.5-2 h.
4. The method for chemical bath deposition of mesoporous tin dioxide thin film according to claim 1, Features: The concentration of the concentrated hydrochloric acid is 0.03-0.15 mol / L; the concentration of the thioglycolic acid is 0.5-2.75 mmol / L.
5. The method for chemical bath deposition of mesoporous tin dioxide thin film according to claim 1, Features: The tin source is stannous chloride and / or stannous chloride dihydrate.
6. A mesoporous tin dioxide film prepared by the method according to claim 1, Features: A mesoporous tin dioxide film with a thickness of 60-200 nm is obtained by the method according to claim 1.
7. An application of the mesoporous tin dioxide film according to claim 6, Features: Application of the mesoporous tin dioxide film in electron transport layer materials for perovskite solar cells.