A kind of etching liquid for precise control of tiny metal Ni mask pattern and its use method
By adjusting the ratio of concentrated nitric acid, water, concentrated hydrochloric acid and hydrogen peroxide, the corrosion rate of the metal Ni mask is controlled, which solves the problem of inappropriate corrosion rate of the mask material during the GaN etching process in MicroLED chip manufacturing, and realizes the micro metal Ni mask Precise control and integrity of membrane graphics.
Patent Information
- Application Number
- CN202211263976.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-17
AI Technical Summary
In the manufacturing process of MicroLED chips, existing mask materials are easily damaged when the GaN etching depth increases, and the corrosion rate of the metal Ni mask is too slow or too fast in normal temperature and humid environments, making it difficult to accurately control the tiny metal Ni mask pattern. corrosion.
Use a corrosive solution composed of concentrated nitric acid, water, concentrated hydrochloric acid and hydrogen peroxide. By adjusting its volume percentage and corrosion time, the corrosion rate of the metal Ni mask is controlled to form a moderate corrosion effect and ensure graphic integrity and boundary clarity.
It achieves precise etching of metal Ni mask patterns with a size less than 20 μm, ensuring that the pattern is complete and has clear boundaries, and solves the problem of jagged patterns caused by too slow or too fast mask etching rates.
Smart Images

Figure CN115679326B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a metal mask etching solution, and in particular to an etching solution for precise control of tiny metal Ni mask patterns for GaN etching in a MicroLED preparation process and a use method thereof. Background Art
[0002] Micro LED refers to a technology that matrices and miniaturizes traditional LEDs. In the manufacturing process of MicroLED chips, inductively coupled plasma dry etching of GaN materials is usually used to form a step structure. This etching method requires the use of a material as an etching mask to protect the material that does not need to be etched and expose the part that needs to be etched, thereby obtaining the designed chip structure.
[0003] The most commonly used mask materials are generally photoresist or a combination mask of silicon oxide and photoresist. However, with the increase in the etching depth requirements of GaN, this mask material can no longer withstand long-term etching, resulting in etching damage to the mask material, which in turn affects the etching of the GaN material. Metal Ni has high hardness, strong etching resistance, and high etching selectivity, and can be used as a mask material for GaN etching. However, due to its good corrosion resistance and the formation of a dense oxide film on the surface of metal Ni in humid air at room temperature, the corrosion rate of dilute hydrochloric acid is too slow, resulting in the inability to etch small-sized metal Ni mask patterns, while the corrosion rate of aqua regia is too fast, which will etch out more jagged metal Ni mask patterns, or even completely corrode the metal Ni mask pattern. Therefore, it is necessary to configure an etching solution with a moderate corrosion rate that can accurately etch tiny metal Ni mask patterns. Summary of the invention
[0004] The first object of the present invention is to provide an etching solution with precise control of tiny metal Ni mask patterns. The etching rate of the etching solution is moderate and can prepare tiny metal Ni mask patterns for GaN etching. The patterns are complete, have clear boundaries and are less than 20 μm in size.
[0005] The second object of the present invention is to provide a method for using an etching solution for accurately controlling a tiny metal Ni mask pattern.
[0006] The first object of the present invention is achieved by:
[0007] A etching solution for precisely controlling tiny metal Ni mask patterns, characterized by being composed of the following concentrated nitric acid, water, concentrated hydrochloric acid, and hydrogen peroxide in percentage by volume, wherein:
[0008] Concentrated nitric acid: 25-30%: Water: 60-65%: Concentrated hydrochloric acid: 4-5%: Hydrogen peroxide: 4-5%.
[0009] The second object of the present invention is achieved by:
[0010] A method for using an etching solution for precisely controlling a tiny metal Ni mask pattern comprises the following steps:
[0011] A. Provide a GaN-based epitaxial wafer;
[0012] B. Soak the epitaxial wafer in a solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1 for 5 minutes to clean the surface impurities;
[0013] C. After filtering, evaporate a metal Ni mask with a thickness of 50-200nm on the epitaxial wafer;
[0014] D. Prepare a photoresist pattern with a size less than 20 μm on the metal Ni mask;
[0015] E. placing the epitaxial wafer with the photoresist pattern in a mixed solution of 25-30% by volume concentrated nitric acid: 60-65% by volume water: 4-5% by volume concentrated hydrochloric acid for 1-2 minutes;
[0016] F. Take out the epitaxial wafer after being corroded in step E, measure 4-5% hydrogen peroxide and pour it into the mixed solution, stir evenly, and then place the epitaxial wafer in the corrosive solution for 1-2 minutes.
[0017] Furthermore, the size of the metal Ni mask pattern after etching is less than 20 μm.
[0018] The corrosion mechanism of the present invention is: metal Ni has good corrosion resistance, and a dense oxide film will be formed on its surface in humid air at room temperature. Therefore, the corrosion rate of dilute hydrochloric acid is too slow, resulting in the failure to etch out a small-sized metal Ni mask pattern, while the corrosion rate of aqua regia is too fast, which will etch out a metal Ni mask pattern with more jagged shapes, or even completely corrode the metal Ni mask pattern. When the prepared sample is placed in a mixed solution of 25-30% by volume of concentrated nitric acid: 60-65% of water: 4-5% of concentrated hydrochloric acid, and the nitric acid and hydrochloric acid therein can provide nitrate ions and chloride ions when corroded for 1-2 minutes. The nitrate ions and chloride ions will adhere to the oxide film and react with the metal Ni, and then combine with the cations of the oxide film to generate soluble nitrates and chlorides, so that the dissolution and repair process of the oxide film on the surface of the metal Ni is destroyed. If it is not controlled at this time, the corrosion rate will be too fast, causing the metal Ni under the tiny photoresist pattern to be eroded, so that the edge of the tiny metal Ni mask pattern after corrosion has more jagged edges. At this time, after adding 4-5% hydrogen peroxide to the above-mentioned etching solution, a large number of tiny bubbles will be formed on the surface of the sample. The large number of tiny bubbles at the edge of the tiny metal Ni mask pattern will continuously squeeze the etching solution, so that a small amount of etching solution evenly contacts the edge of the tiny metal Ni mask pattern, reducing the corrosion rate of the edge of the metal Ni mask pattern and improving the uniformity of the corrosion of the edge of the metal Ni mask pattern, thereby achieving the effect of accurately controlling the corrosion of the tiny metal Ni mask pattern.
[0019] Therefore, the present invention can accurately etch a metal Ni mask pattern with a size less than 20 μm. The pattern after etching is complete and has clear boundaries, which solves the problem of etching a metal Ni mask pattern with more jagged shapes due to the mask etching rate being too slow or too fast during the preparation of the tiny metal Ni mask pattern. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 A schematic diagram of a GaN-based epitaxial wafer provided by the present invention;
[0021] Figure 2 A schematic diagram of the preparation of the metal Ni mask provided by the present invention;
[0022] Figure 3 A schematic diagram of the spin-coated photoresist provided by the present invention;
[0023] Figure 4 A schematic diagram of the preparation of a micro-photoresist pattern of the present invention;
[0024] Figure 5 A schematic diagram of using the etching solution to prepare a micro-patterned metal Ni mask according to the present invention;
[0025] Figure 6 A schematic diagram of removing the photoresist according to the present invention;
[0026] Wherein, the accompanying drawings are marked as follows:
[0027] 101- GaN-based epitaxial wafer, 102- metal Ni mask, 103- photoresist, 104- tiny photoresist pattern, 105- tiny metal Ni mask pattern. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] A etching solution for precisely controlling tiny metal Ni mask patterns, wherein the volume percentages of the etching solution are 25% concentrated nitric acid: 65% water: 5% concentrated hydrochloric acid: 5% hydrogen peroxide.
[0031] Directions:
[0032] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 25% concentrated nitric acid and pour it into a 1000ml beaker, then measure 65% water and pour it into the beaker, then measure 5% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 5% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0033] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a layer of metal Ni mask 102 with a thickness of 50nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 25% concentrated nitric acid, 65% water, and 5% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 5% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0034] Embodiment 2:
[0035] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 27% concentrated nitric acid: 64% water: 4.5% concentrated hydrochloric acid: 4.5% hydrogen peroxide.
[0036] Directions:
[0037] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 27% concentrated nitric acid and pour it into a 1000ml beaker, then measure 64% water and pour it into the beaker, then measure 4.5% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 4.5% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0038] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a layer of metal Ni mask 102 with a thickness of 90nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 27% concentrated nitric acid, 64% water, and 4.5% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 4.5% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0039] Embodiment 3:
[0040] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 29% concentrated nitric acid: 63% water: 4% concentrated hydrochloric acid: 4% hydrogen peroxide.
[0041] Directions:
[0042] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 29% concentrated nitric acid and pour it into a 1000ml beaker, then measure 63% water and pour it into the beaker, then measure 4% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 4% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0043] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a layer of metal Ni mask 102 with a thickness of 130nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 29% concentrated nitric acid, 63% water, and 4% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 4% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0044] Embodiment 4:
[0045] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 26% concentrated nitric acid: 65% water: 4.5% concentrated hydrochloric acid: 4.5% hydrogen peroxide.
[0046] Directions:
[0047] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 26% concentrated nitric acid and pour it into a 1000ml beaker, then measure 65% water and pour it into the beaker, then measure 4.5% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 4.5% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0048] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a metal Ni mask 102 with a thickness of 150nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 26% concentrated nitric acid, 65% water, and 4.5% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 4.5% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0049] Embodiment 5:
[0050] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 28% concentrated nitric acid: 64% water: 4% concentrated hydrochloric acid: 4% hydrogen peroxide.
[0051] Directions:
[0052] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 28% concentrated nitric acid and pour it into a 1000ml beaker, then measure 64% water and pour it into the beaker, then measure 4% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 4% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0053] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a layer of metal Ni mask 102 with a thickness of 160nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 28% concentrated nitric acid, 64% water, and 4% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 4% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0054] Embodiment 6:
[0055] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 30% concentrated nitric acid: 62% water: 4% concentrated hydrochloric acid: 4% hydrogen peroxide.
[0056] Directions:
[0057] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 30% concentrated nitric acid and pour it into a 1000ml beaker, then measure 62% water and pour it into the beaker, then measure 4% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After the sample is placed in the corrosion solution for 1-2 minutes, 4% hydrogen peroxide is poured into the beaker, and the reaction is continued for 1-2 minutes before taking out the sample.
[0058] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a metal Ni mask 102 with a thickness of 180nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 30% concentrated nitric acid, 62% water, and 4% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 4% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0059] Embodiment 7:
[0060] A etching solution for precisely controlling tiny metal Ni mask patterns and a use method thereof, wherein the volume percentages of the etching solution are 30% concentrated nitric acid: 60% water: 5% concentrated hydrochloric acid: 5% hydrogen peroxide.
[0061] Directions:
[0062] When preparing the etching solution for precise control of the tiny metal Ni mask pattern, first measure 30% concentrated nitric acid and pour it into a 1000ml beaker, then measure 60% water and pour it into the beaker, then measure 5% concentrated hydrochloric acid and pour it into the beaker, stir with a glass rod, and Figure 4 After placing the sample in the corrosive solution for 1-2 minutes, 5% hydrogen peroxide is poured into the beaker, and then react for another 1-2 minutes before taking out the sample.
[0063] When using the etching solution with precise control of the tiny metal Ni mask pattern, the metal Ni mask is first prepared, and a GaN-based epitaxial wafer 101 is placed in a solution of concentrated sulfuric acid: hydrogen peroxide equal to 3:1 and immersed for 5 minutes to remove impurities on the surface of the epitaxial wafer, and then the epitaxial wafer 101 is placed in a metal evaporation machine to evaporate a layer of metal Ni mask 102 with a thickness of 200nm, and a layer of photoresist 103 is spin-coated on the surface of the metal Ni mask 102. After photolithography and development, a tiny photoresist pattern 104 is prepared, and then the epitaxial wafer 101 is placed in a mixed solution of 30% concentrated nitric acid, 60% water, and 5% concentrated hydrochloric acid by volume for etching for 1-2 minutes, and then 5% hydrogen peroxide is measured and poured into the beaker, and then reacted for 1-2 minutes to prepare a tiny metal Ni mask pattern 105.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for using an etching solution for precise control of tiny metal Ni mask patterns, characterized in that: The following steps are involved: A. Provide a GaN-based epitaxial wafer; B. Soak the epitaxial wafer in a solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1 for 5 minutes to clean the surface impurities; C. After filtering, evaporate a metal Ni mask with a thickness of 50-200nm on the epitaxial wafer; D. Prepare a photoresist pattern with a size less than 20 μm on the metal Ni mask; E. placing the epitaxial wafer prepared with the photoresist pattern in a mixed solution of 25-30% by volume of concentrated nitric acid, 60-65% by volume of water, and 4-5% by volume of concentrated hydrochloric acid for 1-2 minutes; F. Take out the epitaxial wafer after etching in step E, measure 4-5% by volume of hydrogen peroxide and pour it into the mixed solution to obtain an etching solution, wherein the etching solution is composed of the following concentrated nitric acid, water, concentrated hydrochloric acid, and hydrogen peroxide in volume percentage, wherein: concentrated nitric acid: 25-30%, water: 60-65%, concentrated hydrochloric acid: 4-5%, and hydrogen peroxide: 4-5%; after stirring evenly, place the epitaxial wafer in the etching solution again, and the etching time is 1-2 minutes.