A highly graphitized mesoporous carbon microsphere material and its preparation method and application in electrocatalysis
By inducing sol-gel self-assembly and high-temperature carbonization in a mixed solvent of alcohol and water, highly graphitized mesoporous carbon microspheres were prepared, which solved the problems of insufficient size adjustability and graphitization degree in the existing technology, and achieved High conductivity and widely used in electrocatalysis.
Patent Information
- Application Number
- CN202110836076.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-07-23
AI Technical Summary
It is difficult to prepare monodisperse mesoporous carbon microsphere materials with accurately adjustable sizes in the range of 200-2000 nm using existing technology, and the degree of graphitization is not high, resulting in insufficient conductivity and limiting its application performance in the field of electrocatalysis.
In a mixed solvent of alcohol and water, the sol-gel self-assembly process is induced by adding polymer monomers, organosilane coupling agents and their catalysts, and through high-temperature carbonization and etching treatments, a monodisperse mesoporous structure is formed. Carbon microsphere material with high degree of graphitization.
The preparation of highly graphitized mesoporous carbon microsphere materials has been achieved. It has high conductivity and adjustable particle size. It is suitable for carrier materials in the field of electrocatalysis and improves the performance and application potential of the material.
Smart Images

Figure CN115679359B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material preparation, and specifically relates to a highly graphitized mesoporous carbon microsphere material and a preparation method thereof and application in the field of electrocatalysis. Background Art
[0002] Nano-mesoporous materials have great application prospects in many fields, such as electronic information, environmental protection, catalysis, cosmetics, and medical science, due to their special physical and chemical properties and mesoporous structural characteristics. In the application process, many structural characteristics of the material itself play a decisive role in its performance, such as the composition, dispersibility, particle size, surface state, conductivity and other structural characteristics of the material. With the continuous improvement of the requirements for the application performance of materials, higher requirements are put forward for the material structure design and its preparation control. The preparation and application of size-adjustable mesoporous structure materials have also attracted more and more attention from researchers, especially carbon-based mesoporous nanomaterials have become the research focus of various material application fields. The preparation methods of mesoporous carbon microsphere materials currently developed mainly include template method and microemulsion method, but these preparation processes are usually difficult to prepare monodisperse carbon mesoporous microsphere materials with precisely adjustable sizes in the range of 200-2000nm, and these preparation processes often use organic polymer template agents, which cause more safety or environmental problems. In addition, the prepared hollow carbon microsphere materials often have a relatively small specific surface area, and the degree of graphitization is often not high, resulting in poor conductivity, which greatly limits the improvement of the application performance of mesoporous carbon materials in the field of electrocatalysis. Therefore, the preparation of monodisperse carbon mesoporous microspheres with controllable sizes in a large range is still a great technical challenge. Therefore, it is of great significance to develop a simple preparation method for monodisperse mesoporous carbon microspheres with adjustable diameters in a large range. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a highly graphitized mesoporous carbon microsphere material with simple operation, cheap and readily available raw materials, good repeatability and industrial preparation, as well as its preparation method and application in the field of electrocatalysis.
[0004] To achieve the above purpose, the present invention adopts the following technical solution:
[0005] A highly graphitized mesoporous carbon microsphere material, the microsphere is a mesoporous structure as a whole, the diameter of the microsphere is 200-2000nm, the size of the mesopore is between 2-50nm, and the specific surface area of the microsphere is 100-2000m 2 / g, pore volume is 0.05-0.75cm3 / g, and conductivity is 5-20S / cm.
[0006] It can be seen from the above that the obtained material has a relatively high degree of graphitization and conductivity.
[0007] A method for preparing highly graphitized mesoporous carbon microsphere material:
[0008] In a mixed solvent of alcohol and water, by adding high molecular weight polymerization monomers, organic silane coupling agents and their catalysts, a sol-gel self-assembly process is induced in the system under the action of the catalyst, and the high molecular weight polymerization and silane coupling agent hydrolysis in the system are regulated, and then high-temperature carbonization and etching treatment are performed in an inert atmosphere to form a highly graphitized carbon microsphere material with a monodisperse mesoporous structure.
[0009] Further:
[0010] In a mixed solvent of alcohol and water, by adding high molecular weight polymerization monomers, organic silane coupling agents and polymerization or hydrolysis catalysts, a sol-gel self-assembly process is induced and controlled in the system under the action of the polymerization catalyst, and the kinetics of polymer polymerization growth and silane coupling agent hydrolysis are effectively regulated. After cleaning and drying, the silicon-containing components are directly removed by high-temperature carbonization and etching in an inert atmosphere, thereby forming a highly graphitized carbon microsphere material with a monodisperse mesoporous structure.
[0011] Going a step further:
[0012] (1) dissolving and dispersing the silane coupling agent in a mixed solution of water and organic alcohol, adding a catalyst after dissolution, and stirring the system to form a uniformly dispersed reaction solution system; controlling the hydrolysis reaction time and speed of the silane coupling agent by adjusting the reaction system (the control system is achieved by adjusting the ratio of alcohol and water in the reaction system, the amount of catalyst, and selecting silane coupling agents with different ligands), then adding a polymer monomer to the above colloidal solution, using the catalyst in the system to simultaneously catalyze and promote the polymerization and cross-linking growth of the polymer monomer, so that the two polymerization reactions in the system are carried out alternately to obtain mixed microsphere precursor particles with an interconnected cross-structure, and then standing and aging for 6-24 hours; the obtained gel mixed solution; wherein the molar ratio of the organic alcohol, water, silane coupling agent and polymer monomer used in the reaction system is 10-5000:1-500:0.1-10:1; the volume ratio of the catalyst to the polymer monomer is 1:1-10;
[0013] (2) centrifuging the white polymer gel mixed solution obtained above, washing the precipitate repeatedly with water and organic alcohol, and then drying it to obtain a monodisperse microsphere material;
[0014] (3) subjecting the monodisperse microsphere material obtained above to a high-temperature calcination treatment under an inert atmosphere to obtain a carbon microsphere material with a size adjustable within the range of 200-2000 nm, monodisperse, mesoporous structure, and a high degree of graphitization.
[0015] In step (1), the silane coupling agent is a silicon-containing precursor that can be hydrolyzed in water under catalysis; the organic alcohol solvent is a low-carbon organic alcohol containing a short alkyl chain; the catalytic reaction temperature range of step (1) is 0-100° C., and the entire reaction time is 6-24 hours;
[0016] The organic polymerizable monomer is one of styrene, aniline, pyrrole, pyridine, phenol-formaldehyde, resorcinol-formaldehyde, 3-aminophenol-formaldehyde, hexamethylenetetramine-formaldehyde, melamine-formaldehyde, urea-formaldehyde, dopamine, or any combination thereof.
[0017] The organic silane coupling agent is Si(OR)4 or SiR a (OR)3, wherein R a , R is H, C1-C5 alkyl, C2-C5 alkenyl, C2-C5 alkynyl, benzene, toluene, xylene, mercapto or aniline;
[0018] Among them, R a R may represent a hydrogen atom, or a branched or unbranched, saturated or unsaturated, optionally at least monosubstituted organic hydrocarbon group, for example, R a , R can independently represent methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, etc. The silicon source can be one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate, tetrabutyl orthosilicate, tetraisopropyl orthosilicate, tetra-tert-butyl silicate, or any combination thereof;
[0019] The organic alcohol solvent is one or any combination of methanol, ethanol, n-propanol, isopropanol, and n-butanol;
[0020] The catalyst is an acidic catalyst or a basic catalyst.
[0021] The acid catalyst is one of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, oxalic acid, acetic acid, hydrogen bromide, sodium persulfate, etc., or any combination thereof; the base catalyst is one of ammonia water, sodium hydroxide, potassium hydroxide, urea, hexamethylenetetramine, ethylenediamine, ethanolamine, etc., or any combination thereof.
[0022] The stirring in step (1) is mechanical stirring, with a stirring power range of 20-400W and a stirring speed of 0-300rpm.
[0023] The centrifugal speed of the centrifugal separation in step (2) is 5000-16000 rpm, and the centrifugal time is 3-10 minutes. The solvent selected for the washing is water, ethanol or any combination thereof.
[0024] The calcination is carried out in a tubular furnace at 800-2500° C. for 3-6 hours under a protective atmosphere; the calcination protective atmosphere is one of nitrogen, high-purity nitrogen, and argon hydrogen-argon mixed gas.
[0025] An application of a highly graphitized mesoporous carbon microsphere material, wherein the highly graphitized mesoporous carbon microsphere material is used as a carrier material of an electrocatalyst in the field of electrocatalysis.
[0026] Furthermore, it can be used as a support material for electrocatalysts such as oxygen reduction reaction (ORR), electrocatalytic oxygen evolution reaction (OER), electrocatalytic hydrogen oxidation (HOR), and electrocatalytic hydrogen evolution reaction (HER).
[0027] The mesoporous carbon microspheres provided by the present invention have an overall mesoporous structure, adjustable particle size and mesopore size, and have the characteristics of low cost, uniform overall structure, and high graphitization, and can be used to prepare electrocatalytic support materials. For example, the mesoporous carbon microspheres themselves can be used as catalytic supports to load active components such as metal Pt, Ru, Pt-Co, Ir, etc. to prepare catalysts such as oxygen reduction (ORR), electrocatalytic oxygen evolution (OER), electrocatalytic hydrogen oxidation (HOR), and electrocatalytic hydrogen evolution (HER).
[0028] In the present invention, a silane coupling agent is dissolved and dispersed in a mixed solution of water and an organic alcohol of a certain composition, and an acid or base catalyst is added after the dissolution and stirred to form a uniformly dispersed reaction solution system; on the basis of controlling the hydrolysis reaction time and speed of the silane coupling agent, a high molecular weight polymerization monomer is then added to the above colloidal solution, and the acid or base catalyst in the system is used to simultaneously catalyze and promote the polymerization and cross-linking growth of the high molecular weight polymerization monomer, while the hydrolysis polymerization reaction of the silane coupling agent is also continuing to occur, so that the above two polymerization growth processes can be interactively carried out in space and time, so that mixed microsphere precursor particles with a certain interconnected cross structure can be obtained, which are repeatedly washed with water and organic alcohol, appropriately dried and subjected to high temperature (even 2500 degrees high temperature) carbonization treatment, and the silicon-containing component is etched to remove, so as to obtain a carbon microsphere material with a high degree of graphitization having a monodisperse mesoporous structure with adjustable size in a large range.
[0029] The advantages of the present invention are:
[0030] Compared with the prior art, the present invention achieves effective regulation of the hydrolysis polymerization rate of the organic silane coupling agent in a simple water and alcohol mixed solution by adjusting the ratio of alcohol and water in the reaction system, the amount of catalyst, and selecting silane coupling agents with different ligands, and at the same time introduces an acid or base catalyst that can effectively regulate the organic polymerization monomer. After the organic polymer monomer precursor is added to the system, the organic polymerization monomer precursor and the silane coupling agent can effectively achieve mutual coordination of hydrolysis, cross-linking, polymerization, precipitation and other processes in a water and organic alcohol mixed solvent through the interaction between the organic polymerization monomer precursor and the silane coupling agent hydrolysis oligomer, and self-assemble into monodisperse colloidal microspheres in which the polymer and silicon components are cross-linked, and the colloidal microspheres can be effectively prevented from agglomerating and growing. Subsequently, a water and organic alcohol washing process is adopted, and then drying and high-temperature carbonization treatment are performed to obtain a monodisperse highly graphitized mesoporous carbon microsphere material.
[0031] Compared with the traditional synthesis method, the invented method has strong controllability, simple process, good repeatability, convenient operation, low cost, and does not require the use of corrosive polymer templates. The obtained carbon mesoporous microspheres have a relatively wide and adjustable diameter size (200-2000nm), spherical morphology, good monodispersity, uniform particle size, high specific surface area and porosity, and can be used as an excellent electrocatalytic carrier material. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Characteristic scanning electron microscope (SEM) image of highly graphitized mesoporous carbon microsphere material prepared in Example 1;
[0033] Figure 2 Characteristic transmission electron microscope (TEM) image of highly graphitized mesoporous carbon microspheres prepared in Example 1;
[0034] Figure 3 This is the electrochemical performance curve of the highly graphitized mesoporous carbon microsphere material prepared in Example 1 used as an ORR electrocatalytic carrier loaded with 10 wt% platinum catalyst. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0036] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0037] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0038] Example 1
[0039] (1) 10 g of tetraethyl silicate was dissolved in 100 ml of water and 600 ml of ethanol under stirring. After dissolution, 5 ml of ammonia water was added as a catalyst and mechanical stirring was continued. After stirring for 1 minute, 2 g of resorcinol was added to the mixed solution and stirred to dissolve it. Then 2.8 ml of formaldehyde solution was added dropwise to the solution and stirring was continued for 8 hours to obtain a white gel mixed solution. The entire polymerization reaction process was controlled at room temperature of 25°C.
[0040] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 350 nm.
[0041] (3) Then, after calcination at 1100°C for 4 hours under nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodispersed mesoporous carbon microspheres with a diameter of 300 nm were obtained. The morphology and properties of the microspheres are shown in Figure 1-Figure 3 The prepared carbon microsphere material has a spherical morphology and a mesoporous structure. The diameter of the microsphere is about 300nm. The spherical material has a regular mesoporous structure with a mesopore size of 7-15nm. The monodispersity coefficient can reach 0.15 through dynamic light scattering, and the nitrogen adsorption and desorption test shows that it has a high molecular weight of 980g / m 2 When used as an ORR electrocatalytic support material with 10 wt% Pt loaded, its half-wave potential can be close to 0.89. The linear polarization curve of the oxygen reduction performance test of the prepared catalyst (0.1 M HClO4, O2 saturation) is as follows: Figure 3The electrochemical performance test results of the rotating disk electrode were obtained: the mass specific activity measured at 0.9 V (vs. RHE) was 0.407 A / mgPt.
[0042] Example 2
[0043] (1) 10 g of tetraethyl silicate was dissolved in 70 ml of water and 500 ml of ethanol under stirring. After dissolution, 7 ml of ammonia water was added as a catalyst and mechanical stirring was continued. After stirring for 1 minute, 2 g of resorcinol was added to the mixed solution and stirred to dissolve it. Then 2.8 ml of formaldehyde solution was added dropwise to the solution and stirring was continued for 8 hours to obtain a white gel mixed solution. The entire polymerization reaction process was controlled at room temperature of 25°C.
[0044] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 480 nm.
[0045] (3) After calcination at 1400°C for 4 hours under a nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodisperse mesoporous carbon microspheres with a diameter of 450 nm were obtained.
[0046] Characteristic scanning of the obtained microspheres shows that the product has a carbon microsphere material with a spherical morphology and a mesoporous structure, and the diameter of the microspheres is about 450nm; the spherical material has a regular mesoporous structure, and the mesopore size is 4-10nm.
[0047] Example 3
[0048] (1) 10 g of tetrapropyl silicate was dissolved in 100 ml of water and 600 ml of methanol under stirring. After dissolution, 5 ml of ammonia water was added as a catalyst and mechanical stirring was continued. After stirring for 10 minutes, 2 g of resorcinol was added to the mixed solution and stirred to dissolve it. Then 2.8 ml of formaldehyde solution was added dropwise to the solution and stirring was continued for 8 hours to obtain a white gel mixed solution. The entire polymerization reaction process was controlled at room temperature of 25°C.
[0049] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 380 nm.
[0050] (3) Then, after calcination at 1200°C for 4 hours under nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodispersed mesoporous carbon microspheres with a diameter of 330 nm were obtained. The obtained microspheres were scanned and found to have a spherical morphology and a mesoporous structure. The diameter of the microspheres was about 330 nm. The spherical material had a regular mesoporous structure with a mesopore size of 8-20 nm.
[0051] Example 4
[0052] (1) 10 g of tetrabutyl silicate was dissolved in 100 ml of water and 600 ml of silica under stirring. After dissolution, 5 ml of ammonia water was added as a catalyst and mechanical stirring was continued. After stirring for 10 minutes, 2 g of resorcinol was added to the mixed solution and stirred to dissolve it. Then 2.8 ml of formaldehyde solution was added dropwise to the solution and stirring was continued for 8 hours to obtain a white gel mixed solution. The entire polymerization reaction process was controlled at room temperature of 25°C.
[0053] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 420 nm.
[0054] (3) Then, after calcination at 1400°C for 4 hours under nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodispersed mesoporous carbon microspheres with a diameter of 390 nm were obtained. The obtained microspheres were scanned and found to have a spherical morphology and a mesoporous structure. The diameter of the microspheres was about 390 nm. The spherical material had a regular mesoporous structure with a mesopore size of 10-27 nm.
[0055] Example 5
[0056] (1) 10 g of 1,4-bis(triethoxysilyl)benzene was dissolved in 100 ml of water and 600 ml of isopropanol under stirring. After dissolution, 5 ml of ammonia water was added as a catalyst and mechanical stirring was continued. After stirring for 10 minutes, 2 g of resorcinol was added to the mixed solution and stirred to dissolve it. Then, 2.8 ml of formaldehyde solution was added dropwise to the solution and stirring was continued for 8 hours to obtain a white gel mixed solution. The entire polymerization reaction process was controlled at room temperature of 50°C.
[0057] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 500 nm.
[0058] (3) Then, after calcination at 1200°C for 4 hours under nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodispersed mesoporous carbon microspheres with a diameter of 470 nm were obtained. The obtained microspheres were scanned and found to have a spherical morphology and a mesoporous structure. The diameter of the microspheres was about 470 nm. The spherical material had a regular mesoporous structure with a mesopore size of 6-20 nm.
[0059] Example 6
[0060] (1) 3 g of urea was dissolved in 400 ml of water and 100 ml of methanol under stirring. After the dissolution, 2.8 ml of formaldehyde solution was added dropwise to the above solution. The reaction temperature was controlled to 80° C. Then, 1 ml of formic acid was added to the reaction system as a catalyst. After mechanical stirring was continued for 1 min, 5 g of 1,4-bis(triethoxysilyl)benzene was added to the reaction system. After stirring was continued for 8 h, a white gel mixed solution was obtained.
[0061] (2) The obtained white gel mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the white gel precipitate product, which was then washed three times with ethanol and three times with water. The obtained white precipitate was dried in air at 60°C for 12 hours to obtain monodisperse microspheres with a diameter of 500 nm.
[0062] (3) Then, after calcination at 1200°C for 4 hours under nitrogen atmosphere, the product was treated with 2M NaOH at 60°C for 6 hours and then washed with water three times. After drying, monodispersed mesoporous carbon microspheres with a diameter of 470 nm were obtained. The obtained microspheres were scanned and found to have a spherical morphology and a mesoporous structure. The diameter of the microspheres was about 470 nm. The spherical material had a regular mesoporous structure with a mesopore size of 6-20 nm.
[0063] The morphology and properties of the monodisperse carbon mesoporous microspheres prepared in Examples 2-6 are similar to those in Example 1, and thus they can be used as carrier materials for electrocatalysts such as oxygen reduction (ORR), electrocatalytic oxygen evolution (OER), electrocatalytic hydrogen oxidation (HOR), and electrocatalytic hydrogen evolution (HER) to achieve corresponding effects.
[0064] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A highly graphitized mesoporous carbon microsphere material, Features: The microspheres are mesoporous in structure, with a diameter of 200-2000nm, a mesopore size of 2-50nm, and a specific surface area of 100-2000m 2 / g, pore volume is 0.05-0.75cm3 / g, conductivity is 5-20S / cm; The method for preparing the highly graphitized mesoporous carbon microsphere material is characterized by: (1) dissolving and dispersing a silane coupling agent in a mixed solution of water and an organic alcohol, adding a catalyst after dissolution, and stirring the system to form a uniformly dispersed reaction solution system; controlling the hydrolysis reaction time and speed of the silane coupling agent by adjusting the reaction system, and then adding a polymer monomer to the colloidal solution, using the catalyst in the system to simultaneously catalyze and promote the polymerization and cross-linking growth of the polymer monomer, so that two polymerization reactions in the system are carried out alternately to obtain mixed microsphere precursor particles with an interconnected cross-structure, and then standing and aging for 6-24 hours; the obtained gel mixed solution; wherein the molar ratio of the organic alcohol, water, silane coupling agent and polymer monomer used in the reaction system is 10-5000:1-500:0.1-10:1; the volume ratio of the catalyst to the polymer monomer is 1:1-10; (2) centrifuging the white polymer gel mixed solution obtained in step (1), repeatedly washing the precipitate with water and organic alcohol, and then drying it to obtain a monodisperse microsphere material; (3) subjecting the monodisperse microsphere material obtained above to high temperature calcination and etching treatment under an inert atmosphere to obtain a carbon microsphere material with a size adjustable within the range of 200-2000 nm, monodisperse, mesoporous structure, and high degree of graphitization.
2. A method for preparing the highly graphitized mesoporous carbon microsphere material according to claim 1, Features: (1) dissolving and dispersing a silane coupling agent in a mixed solution of water and an organic alcohol, adding a catalyst after dissolution, and stirring the system to form a uniformly dispersed reaction solution system; controlling the hydrolysis reaction time and speed of the silane coupling agent by adjusting the reaction system, and then adding a polymer monomer to the colloidal solution, using the catalyst in the system to simultaneously catalyze and promote the polymerization and cross-linking growth of the polymer monomer, so that two polymerization reactions in the system are carried out alternately to obtain mixed microsphere precursor particles with an interconnected cross-structure, and then standing and aging for 6-24 hours; the obtained gel mixed solution; wherein the molar ratio of the organic alcohol, water, silane coupling agent and polymer monomer used in the reaction system is 10-5000:1-500:0.1-10:1; the volume ratio of the catalyst to the polymer monomer is 1:1-10; (2) centrifuging the white polymer gel mixed solution obtained in step (1), repeatedly washing the precipitate with water and organic alcohol, and then drying it to obtain a monodisperse microsphere material; (3) subjecting the monodisperse microsphere material obtained above to high temperature calcination and etching treatment under an inert atmosphere to obtain a carbon microsphere material with a size adjustable within the range of 200-2000 nm, monodisperse, mesoporous structure, and high degree of graphitization.
3. The preparation method according to claim 2, It is characterized in that In step (1), the silane coupling agent is a silicon-containing precursor that can be hydrolyzed in water under catalysis; the organic alcohol solvent is a low-carbon organic alcohol containing a short alkyl chain; the catalytic reaction temperature range of step (1) is 0-100° C., and the entire reaction time is 6-24 hours; The organic polymerizable monomer is one of styrene, aniline, pyrrole, pyridine, phenol-formaldehyde, resorcinol-formaldehyde, 3-aminophenol-formaldehyde, hexamethylenetetramine-formaldehyde, melamine-formaldehyde, urea-formaldehyde, dopamine, or any combination thereof.
4. The preparation method according to claim 3, It is characterized in that The organic silane coupling agent is Si(OR) 4 or SiR a (OR)3, wherein R a , R is H, C1-C5 alkyl, C2-C5 alkenyl, C2-C5 alkynyl, benzene, toluene, xylene, mercapto or aniline; The organic alcohol solvent is one or any combination of methanol, ethanol, n-propanol, isopropanol, and n-butanol; The catalyst is an acidic catalyst or a basic catalyst.
5. The preparation method according to claim 4, It is characterized in that The acid catalyst is one of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, oxalic acid, acetic acid, hydrogen bromide, sodium persulfate, etc., or any combination thereof; the base catalyst is one of ammonia water, sodium hydroxide, potassium hydroxide, urea, hexamethylenetetramine, ethylenediamine, ethanolamine, etc., or any combination thereof.
6. The method for preparing the highly graphitized mesoporous carbon microsphere material according to claim 2, It is characterized in that The stirring in step (1) is mechanical stirring, with a stirring power range of 20-400W and a stirring speed of 0-300rpm.
7. The method for preparing the highly graphitized mesoporous carbon microsphere material according to claim 2, It is characterized in that The centrifugal separation in step (2) is carried out at a speed of 5000-16000 rpm and for a time of 3-10 minutes.
8. The preparation method according to claim 2, It is characterized in that The calcination is carried out in a tubular furnace at 800-2500° C. for 3-6 hours under a protective atmosphere; the calcination protective atmosphere is one of nitrogen, high-purity nitrogen, and argon hydrogen-argon mixed gas.
9. An application of the highly graphitized mesoporous carbon microsphere material according to claim 1, It is characterized in that The highly graphitized mesoporous carbon microsphere material is used as a carrier material for electrocatalysts in the field of electrocatalysis.