TFT photoelectric panel and manufacturing method thereof
By removing residual glue and copper particles and foreign matter during the manufacturing process of TFT photovoltaic panels, and controlling the plating and lamination speed, the problems of foreign matter on the board surface and line width burrs are solved, and the impedance stability and yield rate of the photovoltaic panel are improved.
Patent Information
- Application Number
- CN202211296474.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-10-21
AI Technical Summary
During the manufacturing process of TFT photovoltaic panels, there are problems such as serious foreign matter on the board surface, large line width burrs, and poor impedance, resulting in poor yield.
In the process of manufacturing TFT photovoltaic panels, the board body is first inspected and removed for residual glue to ensure that the extreme value of the copper layer after electroplating is within the preset range. After electroplating, copper particles and foreign matter are inspected and removed, and then the copper particles are removed at a predetermined speed. Laminate the dry film, perform exposure, development and negative etching, and finally perform film removal and outer layer etching inspection.
Through these steps, the formability of the copper layer and the stability of the line width are improved, the bonding force between the board and the dry film is enhanced, and the yield of the TFT photovoltaic panel is significantly improved.
Smart Images

Figure CN115692313B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of circuit board processing, and in particular to a TFT photoelectric panel and a manufacturing method thereof. Background Art
[0002] TFT (Thin Film Transistor) photovoltaic panels are used in LCDs. In the production process of TFT photovoltaic panels, due to the high density of the graphic line design of TFT photovoltaic panels, the TFT photovoltaic panels manufactured by the traditional TFT photovoltaic panel manufacturing method have serious foreign matter on the board surface. In addition, due to the large line width burrs of TFT photovoltaic panels, it is easy to have infiltration plating in the gold immersion process, which makes the impedance of TFT photovoltaic panels poor, and further makes the yield of TFT photovoltaic panels poor. Summary of the invention
[0003] The object of the present invention is to overcome the deficiencies in the prior art and provide a TFT photovoltaic panel with a better yield and a manufacturing method thereof.
[0004] The objective of the present invention is achieved through the following technical solutions:
[0005] A method for manufacturing a TFT photoelectric panel, comprising:
[0006] Check the residual glue on the board to be copper-plated;
[0007] If there is residual glue on the board, remove the residual glue on the board;
[0008] Electroplating the plate body so that the copper thickness range of the plate body is less than or equal to a preset range value;
[0009] Inspecting the plate after electroplating for copper particles and foreign matter;
[0010] If there are copper particles on the board surface of the board body, the copper particles on the board surface of the board body are removed;
[0011] Laminating the dry film onto the plate surface of the plate body at a predetermined laminating speed;
[0012] Exposing and developing the pressed plate;
[0013] Performing negative etching on the plate after exposure and development;
[0014] The plate body after the negative film etching is subjected to a film stripping operation to obtain a semi-finished photovoltaic panel;
[0015] The photovoltaic panel semi-finished product is subjected to outer layer corrosion inspection.
[0016] In one embodiment, the preset range value is less than or equal to 6 μm.
[0017] In one of the embodiments, the preset range value is equal to 5 μm.
[0018] In one embodiment, the predetermined lamination speed is less than or equal to 3 m / min.
[0019] In one embodiment, the step of inspecting the residual glue on the board to be copper-plated includes:
[0020] Capturing images of the board to be copper-plated to obtain actual image data of the board;
[0021] Performing fitting processing on the actual image data of the plate to obtain an actual three-dimensional image of the plate;
[0022] Comparing the actual three-dimensional image of the plate with the target three-dimensional image, and calculating the actual deviation value of the plate;
[0023] Determining whether the actual deviation value of the plate is less than or equal to the ideal deviation value;
[0024] If so, there is residual glue on the board.
[0025] In one embodiment, the step of inspecting the copper particles and foreign bodies on the plate after electroplating is specifically as follows:
[0026] The plate body after electroplating is inspected for copper particles and foreign matter by using foreign matter detection equipment.
[0027] In one embodiment, the step of removing the residual glue from the board is specifically:
[0028] The plate body is subjected to a grinding and brushing treatment at a preset grinding speed.
[0029] In one of the embodiments, the preset grinding plate speed is less than or equal to 3 m / min.
[0030] In one of the embodiments, the current for brushing the plate body at a preset grinding speed is less than or equal to 0.3A.
[0031] A TFT photoelectric panel is manufactured by using the manufacturing method of the TFT photoelectric panel described in any of the above embodiments.
[0032] Compared with the prior art, the present invention has at least the following advantages:
[0033] 1. The manufacturing method of the TFT optoelectronic panel mentioned above is that before the electroplating of the panel, the panel is first inspected for residual glue. If there is residual glue on the panel, the residual glue on the panel is removed, so that the copper layer of the electroplating process is better formed on the panel surface of the panel. At the same time, when the panel is electroplated, the copper thickness range of the panel is less than or equal to the preset range value, so that the burrs of the line width after subsequent etching are less than the preset value, thereby improving the impedance stability of the TFT optoelectronic panel;
[0034] 2. Since the board is inspected for copper particles after electroplating, if there are copper particles on the board surface, the copper particles on the board surface are removed, which improves the adhesion between the board and the dry film, thereby improving the bonding strength between the board and the dry film. Moreover, since the dry film is pressed onto the board surface of the board at a predetermined film pressing speed, compared with the traditional TFT photovoltaic panel manufacturing method, the bonding strength between the board and the dry film is further improved, thereby improving the yield of the TFT photovoltaic panel. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 A schematic diagram of a process for manufacturing a TFT photovoltaic panel according to an embodiment of the present invention;
[0037] Figure 2 A schematic structural diagram of a developing tank line of a method for manufacturing a TFT photovoltaic panel according to an embodiment;
[0038] Figure 3 for Figure 2 A schematic diagram of a movable pressing plate of a mounting frame of the developer tank line shown;
[0039] Figure 4 for Figure 2 A partial schematic diagram of another viewing angle of the developing tank line shown;
[0040] Figure 5 for Figure 2 A partial schematic diagram of the conveying roller assembly of the developer tank line shown. DETAILED DESCRIPTION
[0041] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0042] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0044] The present application also provides a method for manufacturing a TFT optoelectronic panel, comprising: inspecting a board to be copper-plated for residual glue; if residual glue exists on the board, removing the residual glue from the board; electroplating the board so that the copper thickness range of the board is less than or equal to a preset range; inspecting the electroplated board for copper particles; if copper particles exist on the board surface of the board, removing the copper particles on the board surface of the board; pressing a dry film onto the board surface of the board at a predetermined film pressing speed; exposing and developing the pressed board; negatively etching the board after exposure and development; stripping the board after negative film etching to obtain a semi-finished optoelectronic panel; and performing an outer layer etching inspection on the semi-finished optoelectronic panel.
[0045] The above-mentioned manufacturing method of the TFT optoelectronic panel is that before the electroplating of the panel, the panel is first inspected for residual glue. If there is residual glue on the panel, the residual glue on the panel is removed, so that the copper layer of the electroplating process is better formed on the board surface of the panel. At the same time, when the panel is electroplated, the copper thickness range of the panel is less than or equal to the preset range, so that the burrs of the line width after subsequent etching are less than the preset value, thereby improving the impedance stability of the TFT optoelectronic panel; after the electroplating, the panel is also inspected for copper particles and foreign matter. If there are copper particles and foreign matter on the board surface of the panel, the copper particles and foreign matter on the board surface of the panel are removed, thereby improving the adhesion between the panel and the dry film, thereby improving the bonding strength between the panel and the dry film, and since the dry film is pressed onto the board surface of the panel at a predetermined film pressing speed, compared with the traditional manufacturing method of the TFT optoelectronic panel, the bonding strength between the panel and the dry film is further improved, thereby improving the yield rate of the TFT optoelectronic panel.
[0046] In order to better understand the technical solution of the present application, the technical solution of the present application is further explained as follows:
[0047] like Figure 1 As shown, a method for manufacturing a TFT optoelectronic panel in an embodiment is used to manufacture a TFT optoelectronic panel. Further, the method for manufacturing a TFT optoelectronic panel includes some or all of the following steps:
[0048] S101, inspect the residual glue on the board to be copper plated.
[0049] In this embodiment, the board to be copper-plated is inspected for residual glue. Before the board is electroplated, the board is inspected for residual glue to prevent residual glue on the board from affecting the quality of subsequent copper deposition.
[0050] S103: If there is residual glue on the board, remove the residual glue on the board.
[0051] In this embodiment, if there is residual glue on the board, the residual glue on the board is removed so that the copper layer in the electroplating process can be better formed on the board surface of the board.
[0052] S105, electroplating the plate body so that the copper thickness range of the plate body is less than or equal to a preset range value.
[0053] In this embodiment, the plate is electroplated so that the copper thickness range of the plate is less than or equal to a preset range value, that is, when the plate is electroplated, the copper thickness range of the plate is controlled to be less than or equal to the preset range value, so that the burrs of the line width after subsequent etching are less than a predetermined value, thereby improving the impedance stability of the TFT photoelectric panel. In addition, before electroplating, the residual glue inspection and removal operations of the plate are first performed, which is conducive to the reliable control of the copper thickness range of the plate, so that the copper thickness range of the plate is controlled to be less than or equal to the preset range value.
[0054] S107, inspecting the plate body after electroplating for copper particles and foreign matter.
[0055] In this embodiment, the plate body after electroplating is inspected for copper particles and foreign matter, so as to prevent the copper particles and foreign matter on the plate body from affecting the bonding force with the subsequent dry film pressing.
[0056] S109, if there are copper particles on the board surface of the board, the copper particles on the board surface are removed.
[0057] In this embodiment, if there are copper particles on the board surface of the board, the copper particles on the board surface are removed to make the board surface smoother and make the dry film better fit to the board surface.
[0058] S111, pressing the dry film onto the board surface of the board body at a predetermined film pressing speed.
[0059] In this embodiment, the dry film is pressed onto the board surface of the board body at a predetermined film pressing speed, so that the dry film is better attached to the board surface of the board body.
[0060] S113, exposing and developing the laminated plate.
[0061] In this embodiment, the laminated plate is exposed and developed, so that the dry film to be retained is hardened by chemical action of the dry film resist under the light, so that the unhardened dry film can be washed away in the development process.
[0062] S115, negative etching is performed on the plate after exposure and development.
[0063] In this embodiment, the board after exposure and development is negatively etched, that is, the copper foil portion of the dry film washed away of the board after exposure and development is bitten, and then the copper foil portion of the dry film not washed away is retained to obtain the circuit required for the board.
[0064] S117, performing a film stripping operation on the plate body after the negative film is etched to obtain a semi-finished photovoltaic panel.
[0065] In this embodiment, the plate body after negative film etching is subjected to a film stripping operation, that is, the dry film of the plate body is removed to expose the copper deposited on the plate surface, thereby obtaining a semi-finished photovoltaic panel.
[0066] S119, performing outer layer etching inspection on the semi-finished photovoltaic panel.
[0067] In this embodiment, the outer layer of the photovoltaic panel semi-finished product is subjected to an etching inspection so as to make further repairs.
[0068] The above-mentioned method for manufacturing the TFT optoelectronic panel is that before the electroplating of the panel, the panel is first inspected for residual glue. If there is residual glue on the panel, the residual glue on the panel is removed, so that the copper layer of the electroplating process is better formed on the surface of the panel. At the same time, when the panel is electroplated, the range of the copper thickness of the panel is less than or equal to the preset range, so that the burrs of the line width after subsequent etching are less than the preset value, thereby improving the impedance stability of the TFT optoelectronic panel; further, since the panel is also inspected for copper particles after electroplating, if there are copper particles on the surface of the panel, the copper particles on the surface of the panel are removed, thereby improving the adhesion between the panel and the dry film, thereby improving the bonding strength between the panel and the dry film, and since the dry film is pressed onto the surface of the panel at a predetermined film pressing speed, compared with the traditional method for manufacturing the TFT optoelectronic panel, the bonding strength between the panel and the dry film is further improved, thereby improving the yield rate of the TFT optoelectronic panel.
[0069] In one embodiment, the preset range is less than or equal to 6 μm, so that the copper thickness range of the board meets the better impedance performance requirements of the TFT optoelectronic board. In one embodiment, the preset range is equal to 5 μm, so that the manufactured TFT optoelectronic board has more stable impedance performance and can ensure that the line width burrs are small after etching.
[0070] In one embodiment, the predetermined lamination speed is less than or equal to 3 m / min, so that the speed during the lamination operation is relatively low, thereby enabling the plate body and the dry film to be better combined after the lamination operation.
[0071] Furthermore, after the step of laminating the dry film onto the surface of the board at a predetermined laminating speed, and before the step of exposing and developing the laminated board, the method for manufacturing the TFT optoelectronic panel also includes: detecting the flatness of the surface of the laminated board; if the flatness of the surface of the board is less than the predetermined flatness, adjusting the predetermined laminating speed to reduce the predetermined laminating speed to 0.8 times the predetermined laminating speed, so that the surface of the laminated board has better flatness, and the dry film is better laminated onto the surface of the board after laminating.
[0072] In one embodiment, the step of inspecting the residual glue on the plate to be copper-plated includes: firstly, performing image acquisition on the plate to be copper-plated to obtain the actual image data of the plate; then performing fitting processing on the actual image data of the plate to obtain the actual three-dimensional image of the plate; then comparing the actual three-dimensional image of the plate with the target three-dimensional image, and calculating the actual deviation value of the plate; judging whether the actual deviation value of the plate is less than or equal to the ideal deviation value; if so, there is residual glue on the plate, and automatic visual inspection of the residual glue is realized, which improves the inspection efficiency and accuracy of the residual glue compared with the traditional manual inspection. In this embodiment, before the step of performing image acquisition on the plate to be copper-plated to obtain the actual image data of the plate, the step of inspecting the residual glue on the plate to be copper-plated also includes: establishing a database of one-to-one correspondence between multiple models of plates and multiple ideal deviation values; retrieving the target model of the plate and the corresponding ideal deviation value, which improves the applicability of the step of inspecting the residual glue on the plate to be copper-plated.
[0073] In one of the embodiments, the step of inspecting the plate body for copper particles after electroplating is specifically as follows: inspecting the plate body for copper particles after electroplating by means of a foreign matter detection device, thereby improving the efficiency and comprehensiveness of the inspection of copper particles. In this embodiment, the foreign matter detection device may be a visual aid device. For example, the visual aid device may be a magnifying glass or other auxiliary equipment. Specifically, the visual aid device may be a 40x magnifying glass. Furthermore, inspecting the plate body for copper particles after electroplating by means of a foreign matter detection device includes: firstly, performing a roughness detection operation on the surface of the plate body by means of a sensing element; then, if the sensing element detects that the surface roughness of the plate body is greater than a preset roughness, defining the surface of the plate body as an observation area; finally, performing a copper particle foreign matter inspection operation on the surface of the plate body by means of a visual aid device, thereby improving the efficiency of the inspection of copper particles of the plate body.
[0074] In one embodiment, the step of removing the residual glue on the plate body is specifically: grinding and brushing the plate body at a preset grinding speed to remove the residual glue on the surface of the plate body. In one embodiment, the preset grinding speed is less than or equal to 3m / min, so that the residual glue on the surface of the plate body can be better removed.
[0075] Furthermore, before the step of inspecting the residual glue on the copper-plated board, the manufacturing method further includes: etching the board through the micro-etching section. Furthermore, before the step of etching the board through the micro-etching section, the manufacturing method further includes: increasing the concentration and temperature of the solution in the micro-etching section to increase the etching rate on the board surface so that the board achieves a better roughness, thereby achieving better adhesion between the dry film and the board during the dry film application operation.
[0076] However, if the current used for brushing the plate body is too large, it will cause the problem of excessive expansion and contraction; if the current used for brushing the plate body is too small, it will cause serious foreign matter on the plate surface. In one embodiment, the current used for brushing the plate body at a preset grinding speed is less than or equal to 0.3A, while the current used for brushing the plate body in the conventional method is 0.12A to 0.13A. The current used for brushing the plate body in the present application is relatively large, which improves the effect of removing residual glue from the plate body, thereby improving the cleaning effect of the plate body, and at the same time avoids the problem of causing a large expansion and contraction effect. In this embodiment, the preset grinding speed is less than or equal to 3m / min, and the current used for brushing the plate body at the preset grinding speed is less than or equal to 0.3A, which improves the effect of removing residual glue from the plate body, thereby improving the cleaning effect of the plate body, and at the same time avoids the problem of causing a large expansion and contraction effect. In this embodiment, the current for grinding and brushing the plate at a preset grinding speed is less than or equal to 0.3 A, and the current for grinding and brushing the plate at a preset grinding speed is greater than or equal to 0.18 A. After multiple tests and certifications, foreign matter on the plate surface can be greatly reduced, the ratio is reduced from 6.8% to 1.3%, and the short circuit defect rate is improved by 5.2%.
[0077] Furthermore, the step of laminating the dry film onto the board surface of the board body at a predetermined laminating speed is specifically: laminating the dry film onto the board surface of the board body at a predetermined laminating speed by a laminating machine.
[0078] Furthermore, the step of exposing and developing the laminated plate body is specifically: exposing and developing the laminated plate body by an exposure machine.
[0079] Furthermore, the step of performing negative film etching on the plate body after exposure and development is specifically: performing negative film etching on the plate body after exposure and development through etching lines.
[0080] Furthermore, before the step of laminating the dry film onto the board surface of the board body at a predetermined laminating speed, the manufacturing method also includes: cleaning the laminator, exposure machine and etching line respectively, and cleaning the positions where the laminator, exposure machine and etching line contact the board body, so as to better remove foreign matter on the board surface, such as copper particles.
[0081] Furthermore, before the step of exposing and developing the pressed plate, the manufacturing method also includes: taking out the conveying roller corresponding to the nozzle in the developing tank line, so that there is no conveying roller at the position corresponding to the nozzle in the developing tank line while ensuring smooth conveyance of the plate in the developing tank line, so that the developer is more evenly distributed on the surface of the photosensitive dry film, so that the developer can better react on the photosensitive dry film, thereby achieving a better development effect, reducing the problem of residual copper caused by unclean development, and effectively improving the production yield of the TFT photovoltaic panel.
[0082] like Figures 2 to 4 As shown, further, the developer tank line 10 includes a fence 100, a protective door 200, a mounting frame 300, a developer injection assembly 400 and a conveying roller assembly 500, the fence 100 is formed with a connected receiving cavity 103 and a debugging window 105, and the protective door 200 is movably connected to the debugging window 105. The mounting frame 300 is located in the receiving cavity 103 and is connected to the fence 100. See also Figure 5 The conveying roller assembly 500 includes a conveying roller shaft 510 and a plurality of conveying rollers 520. Both ends of the conveying roller shaft 510 are rotatably connected to the mounting frame 300. The plurality of conveying rollers 520 are arranged at intervals along the axial direction of the conveying roller shaft 510. When the conveying roller assembly 500 needs to be debugged or maintained, the protective door 200 is opened, which is convenient and quick. The developer spray assembly 400 is installed on the fence 100, and the spray port of the developer spray assembly 400 is located in the receiving chamber 103, and the spray port of the developer spray assembly 400 is located above the conveying roller assembly 500. The spray port of the developer spray assembly 400 is staggered with each conveying roller 520, that is, the projection of the developer spray assembly 400 on the mounting frame 300 and the projection of each conveying roller 520 in the vertical direction of the mounting frame 300 do not overlap, that is, the spray port of the developer spray assembly 400 is not directly opposite to each conveying roller 520, so that the developer is more evenly distributed on the surface of the photosensitive dry film, so that the developer can better react on the photosensitive dry film, achieve a better development effect, reduce the problem of residual copper caused by unclean development, and effectively improve the production yield of the TFT photovoltaic panel. In this embodiment, the conveying roller assembly 500 further includes a driving assembly 530, a driving gear set 540 and a driven gear 550. The driving assembly 530 is arranged on the mounting frame 300, and the driven gear 550 is sleeved on the conveying roller shaft 510. The power output end of the driving assembly 530 is connected to the driving gear set 540, and the driving gear set 540 and the driven gear 550 are meshed and driven, so that the driving assembly 530 drives the driven gear 550 through the driving gear set 540 to drive the conveying roller shaft 510 to rotate relative to the mounting frame 300. Further, the driving gear set 540 includes two bevel gears meshing with each other, one of which meshes with the driven gear, and the driven gear 550 is a cylindrical gear.
[0083] like Figure 1As shown, further, the developer spray assembly 400 is slidably mounted on the top of the fence 100, so that the mounting position of the developer spray assembly 400 and the fence 100 is adjustable, and the developer spray assembly 400 is detachably connected to the fence 100. In this embodiment, the number of developer spray assemblies 400 is multiple, and the multiple developer spray assemblies 400 are arranged at intervals on the top of the fence 100. Specifically, the multiple developer spray assemblies 400 are arranged in a rectangular array, so that the multiple developer spray assemblies 400 have a better spraying effect. In actual use, the mounting position of the developer spray assembly 400 and the fence 100 can be flexibly adjusted as needed, and the number of developer spray assemblies 400 can be flexibly increased or decreased. Furthermore, a linear slide groove is opened on the top of the fence 100, and the developer spray assembly 400 is located in the linear slide groove and is slidably connected to the fence 100, so that the developer spray assembly 400 is slidably set on the top of the fence 100. In this embodiment, the developer injection assembly 400 includes an injection head 410 and a locking adjustment ring 420. The injection head is inserted into the linear slide groove and is slidably connected to the fence 100. The injection head 410 is convexly provided with a limiting flange 412, and the limiting flange abuts against one side of the fence 100. The outer peripheral wall of the injection head is provided with an external thread, and the locking adjustment ring is formed with an internal thread. The locking adjustment ring is sleeved on the outer peripheral wall of the injection head, and the locking adjustment ring is threadedly connected to the injection head. When it is necessary to adjust the installation position of the injection head relative to the fence 100, the locking adjustment ring is loosened to make the injection head slide relative to the linear slide groove, so that the injection head can better adapt to the development needs of different types of TFT photoelectric panels, thereby improving the applicability of the developing tank line 10.
[0084] like Figure 2 and Figure 4 As shown, further, the mounting frame 300 is provided with a first rotation slot 302 and a second rotation slot 304, and the two ends of the conveying roller shaft 510 are respectively located in the first rotation slot and the second rotation slot and are rotatably connected to the mounting frame 300, so that the two ends of the conveying roller shaft 510 are rotatably connected to the mounting frame 300. In this embodiment, the first rotation slot and the second rotation slot are both rectangular rotation slots. During installation, one end of the conveying roller shaft 510 is first inserted into the first rotation slot, and the other end of the conveying roller shaft 510 is inserted into the second rotation slot, and then the driven gear 550 is sleeved on the conveying roller shaft 510, so as to quickly disassemble and assemble the conveying roller 520 on the conveying roller shaft 510.
[0085] like Figures 2 to 4As shown, further, the mounting frame 300 includes a mounting frame body 310 and a movable pressure plate 320, the first rotating slot and the second rotating slot are both formed on the mounting frame body 310, and the mounting frame body 310 is also provided with a stop opening 306 connected to the first rotating slot 302, one end of the movable pressure plate 320 is rotatably connected to the mounting frame body 310, and the other end of the movable pressure plate 320 is detachably connected to the mounting frame body 310, so that the movable pressure plate 320 is covered on the stop opening, when the conveying roller needs to be removed, the other end of the movable pressure plate 320 is removed from the mounting frame body 310, and the movable pressure plate 320 is rotated by a predetermined angle, so that one end of the conveying roller can be taken out from the stop opening, and then the other end of the conveying roller can be taken out from the second rotating slot. In this embodiment, the driven gear 550 is sleeved on one side of the conveying roller adjacent to the first rotating notch, so as to facilitate the removal of the conveying roller assembly 500, so as to facilitate the quick removal of each conveying roller 520, thereby improving the efficiency of removing the conveying roller 520 corresponding to the nozzle in the developing tank line 10. Furthermore, the other end of the movable pressing plate 320 is buckled on the mounting frame 310, so that the movable pressing plate 320 is detachably connected to the mounting frame 310. In this embodiment, the movable pressing plate 320 is convexly provided with a buckle protrusion 322, and the mounting frame 310 is provided with a buckle groove 312, and the buckle protrusion is snapped into the buckle groove, so that the movable pressing plate 320 is buckled with the mounting frame 310.
[0086] The present application also provides a TFT optoelectronic panel, which is prepared by the manufacturing method of the TFT optoelectronic panel described in any of the above embodiments. Furthermore, the manufacturing method of the TFT optoelectronic panel includes: inspecting the board to be copper-plated with residual glue; if there is residual glue on the board, removing the residual glue on the board; electroplating the board so that the copper thickness range of the board is less than or equal to the preset range; inspecting the electroplated board for copper particles; if there are copper particles on the board surface of the board, removing the copper particles on the board surface of the board; pressing the dry film on the board surface of the board at a predetermined film pressing speed; exposing and developing the pressed board; performing negative film etching on the board after exposure and development; performing film stripping on the board after negative film etching to obtain a semi-finished optoelectronic panel; performing outer layer etching inspection on the semi-finished optoelectronic panel.
[0087] The above-mentioned TFT optoelectronic panel is inspected for residual glue before electroplating the panel. If there is residual glue on the panel, the residual glue on the panel is removed, so that the copper layer of the electroplating process is better formed on the surface of the panel. At the same time, when the panel is electroplated, the copper thickness range of the panel is less than or equal to the preset range, so that the burrs of the line width after subsequent etching are less than the preset value, thereby improving the impedance stability of the TFT optoelectronic panel; after electroplating, the panel is also inspected for copper particles and foreign matter. If there are copper particles and foreign matter on the surface of the panel, the copper particles and foreign matter on the surface of the panel are removed, thereby improving the adhesion between the panel and the dry film, thereby improving the bonding strength between the panel and the dry film, and since the dry film is pressed onto the surface of the panel at a predetermined film pressing speed, compared with the traditional TFT optoelectronic panel manufacturing method, the bonding strength between the panel and the dry film is further improved.
[0088] Compared with the prior art, the present invention has at least the following advantages:
[0089] 1. The manufacturing method of the TFT optoelectronic panel mentioned above is that before the electroplating of the panel, the panel is first inspected for residual glue. If there is residual glue on the panel, the residual glue on the panel is removed, so that the copper layer of the electroplating process is better formed on the panel surface of the panel. At the same time, when the panel is electroplated, the copper thickness range of the panel is less than or equal to the preset range value, so that the burrs of the line width after subsequent etching are less than the preset value, thereby improving the impedance stability of the TFT optoelectronic panel;
[0090] 2. Since the board is inspected for copper particles after electroplating, if there are copper particles on the board surface, the copper particles on the board surface are removed, which improves the adhesion between the board and the dry film, thereby improving the bonding strength between the board and the dry film. Moreover, since the dry film is pressed onto the board surface of the board at a predetermined film pressing speed, compared with the traditional TFT photovoltaic panel manufacturing method, the bonding strength between the board and the dry film is further improved, thereby improving the yield of the TFT photovoltaic panel.
[0091] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for manufacturing a TFT photovoltaic panel, It is characterized in that include: Check the residual glue on the board to be copper-plated; If there is residual glue on the board, remove the residual glue on the board; Electroplating the plate body so that the copper thickness range of the plate body is less than or equal to a preset range value; Inspecting the plate after electroplating for copper particles and foreign matter; If there are copper particles on the board surface of the board body, the copper particles on the board surface of the board body are removed; Laminating the dry film onto the plate surface of the plate body at a predetermined laminating speed; Exposing and developing the pressed plate; Performing negative etching on the plate after exposure and development; The plate body after the negative film etching is subjected to a film stripping operation to obtain a semi-finished photovoltaic panel; The photovoltaic panel semi-finished product is subjected to outer layer etching inspection.
2. The method for manufacturing a TFT photovoltaic panel according to claim 1, It is characterized in that The preset extreme difference value is less than or equal to 6 μm.
3. The method for manufacturing a TFT photovoltaic panel according to claim 2, It is characterized in that The preset extreme difference value is equal to 5 μm.
4. The method for manufacturing a TFT photovoltaic panel according to claim 1, It is characterized in that The predetermined film pressing speed is less than or equal to 3 m / min.
5. The method for manufacturing a TFT photovoltaic panel according to claim 1, It is characterized in that The steps for checking residual glue on the copper-plated board include: Capturing images of the board to be copper-plated to obtain actual image data of the board; Performing fitting processing on the actual image data of the plate to obtain an actual three-dimensional image of the plate; Comparing the actual three-dimensional image of the plate with the target three-dimensional image, and calculating the actual deviation value of the plate; Determining whether the actual deviation value of the plate is less than or equal to the ideal deviation value; If so, there is residual glue on the board.
6. The method for manufacturing a TFT photovoltaic panel according to claim 1, It is characterized in that The specific steps of inspecting the copper particles and foreign bodies on the plate after electroplating are as follows: The plate body after electroplating is inspected for copper particles and foreign matter by using foreign matter detection equipment.
7. The method for manufacturing a TFT photovoltaic panel according to claim 1, It is characterized in that The specific steps of removing the residual glue from the board are: The plate body is subjected to a grinding and brushing treatment at a preset grinding speed.
8. The method for manufacturing a TFT photovoltaic panel according to claim 7, It is characterized in that The preset grinding plate speed is less than or equal to 3 m / min.
9. The method for manufacturing a TFT photovoltaic panel according to claim 7 or 8, It is characterized in that The current for brushing the plate body at a preset grinding speed is less than or equal to 0.3A.
10. A TFT photoelectric panel, It is characterized in that The TFT photovoltaic panel is prepared by the manufacturing method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Electroplating method of circuit board with surface coated with resin
CN103068163A
Method for electroplating circuit board
CN108966517A