A high yield strength continuously wound unsaturated polyester resin and preparation method thereof

By introducing PET crystalline chain segments into the fiberglass wound pipe resin, the heat resistance and high-temperature compression strength of the resin are improved, and the problem that traditional resins are easily damaged during the cooling stage is solved, and matching with the continuous winding molding process is achieved. Improve product quality and production efficiency.

CN115746211BActive Publication Date: 2024-11-22CHANGZHOU RIXIN RESIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211313218.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-11-22
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Traditional fiberglass winding pipeline resin is easily damaged and cracked by guide wheels during the cooling stage, resulting in poor product quality and improving production efficiency methods will reduce the resin's heat resistance and high-temperature compression strength.

Method used

The high yield strength continuous winding of unsaturated polyester resin is adopted. By introducing PET crystalline segments into the resin, the heat resistance and high-temperature compression performance of the resin are improved. The degree of PET alcoholylation is controlled by using an alcoholylation reaction, combining styrene diluent and Zinc acetate catalyst, resin with high heat resistance and high temperature compression strength was prepared.

Benefits of technology

It solves the problem of easy cracking and rolling in the cooling stage of the pipeline, improves the heat resistance and high-temperature compression strength of the resin, is suitable for continuous winding forming process, and improves product quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention relates to the technical field of unsaturated polyester resin, in particular to a high yield strength continuously wound unsaturated polyester resin and a preparation method thereof; the composition by weight is as follows: 20-25 parts of maleic anhydride MA, 20-30 parts of PET, 20-25 parts of diols, 25-30 parts of diluents, 0.02-0.06wt% of catalyst, and 0.01-0.05wt% of polymerization inhibitor; the unsaturated resin material prepared by the present invention introduces PET crystalline segments by controlling the degree of PET alcoholysis reaction, thereby improving the heat resistance and high temperature compression performance of the resin. The unsaturated resin prepared by the present invention has high heat resistance and high temperature compression strength, solves the problems of easy cracking and rolling of the pipeline in the cooling stage of continuous winding pipeline production, and perfectly matches the continuous winding molding process of glass fiber reinforced plastic pipeline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of unsaturated polyester resins, in particular to a high-yield strength continuously wound unsaturated polyester resin and a preparation method thereof. Background Art

[0002] FRP pipes are widely used in oilfield gathering and transportation pipelines and municipal water supply and drainage pipelines because of their light weight, high strength, easy design and molding, anti-aging, anti-freezing, corrosion resistance, wear resistance and high toughness. FRP pipes are processed by fixed-length reciprocating winding process, which has defects such as many processes, low efficiency and poor quality. The continuous winding molding process is a new process developed on the basis of the winding process. It uses a cam disk to drive the steel belt to run continuously to form a pipe winding inner core mold. The steel belt circulates back and forth to complete the fiber winding, compounding, sand inclusion and curing processes on the moving inner core mold. After curing, it is cooled and cut into finished products. This process is continuous molding, which can improve production efficiency and reduce resource waste.

[0003] In order to ensure production efficiency, the continuous winding pipe has a fast pipe output speed, and the molding process requires fast curing and good product quality. However, the traditional fiberglass winding pipe resin is often crushed, embossed, and cracked by the guide wheel during the cooling stage, resulting in poor product quality. This is mainly due to the fast pipe output speed, the cooling stage after curing and exothermic still has a high temperature, and the contact with the guide wheel still needs high strength. The traditional winding pipe resin has low heat resistance and low compression strength at high temperature, and is easily crushed and cracked after contacting the guide wheel.

[0004] The current solutions are: (1) increasing the double bond content of the resin to enhance the crosslinking density of the curing and improve the high temperature compressive strength. However, the increase in the double bond content of the resin will cause faster heat release during curing, a higher heat release peak, and easy cracking during cooling; (2) slowing down the pipe discharge speed to allow for more complete cooling, a lower temperature at the guide wheel, and higher compressive strength. However, the speed reduction will reduce production efficiency and fail to give full play to the advantages of continuous winding equipment. Summary of the invention

[0005] The purpose of the present invention is to provide a high yield strength continuously wound unsaturated polyester resin and a preparation method thereof, so as to solve at least one of the above technical problems.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A high yield strength continuously wound unsaturated polyester resin, the composition by weight is as follows:

[0008] The catalyst is added in an amount of 0.02-0.06% of the total weight of the unsaturated polyester resin.

[0009] The amount of the polymerization inhibitor added is 0.01-0.05% of the total weight of the unsaturated polyester resin.

[0010] Furthermore, the molar ratio of maleic anhydride to diol is 1:1.

[0011] Furthermore, the diol is selected from one or more of propylene glycol, ethylene glycol, diethylene glycol, dipropylene glycol, and neopentyl glycol.

[0012] Furthermore, the PET is PET polyester chips, PET bottle chips and PET materials recycled in daily life.

[0013] Furthermore, the diluent is styrene.

[0014] Furthermore, the catalyst is zinc acetate.

[0015] Furthermore, the polymerization inhibitor is selected from one of hydroquinone HQ, methyl hydroquinone THQ and p-benzoquinone PBQ.

[0016] A method for preparing a high yield strength continuously wound unsaturated polyester resin, the method comprising the following steps: S1, adding a diol, PET and a catalyst into a reaction kettle, introducing nitrogen, stirring, heating to 180°C at 50°C / hour, then raising the kettle temperature to 220±5°C at 15°C / hour, fully reflux and heat preservation, sampling and testing every 1h until the sample: propylene glycol monomethyl ether (RX-064) = 1-1.5 is completely clarified after being mixed, and the sample: methanol = 0.5-1.2 is turbid after mixing and cooling begins, and the temperature drops by 150°C;

[0017] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0018] S3: adding the reactants into the diluent and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0019] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0020] The beneficial effects of the technical solution of the present invention are:

[0021] The unsaturated resin material prepared by the present invention introduces PET crystalline segments by controlling the degree of PET alcoholysis reaction, thereby improving the heat resistance and high-temperature compression performance of the resin.

[0022] The unsaturated resin prepared by the present invention has high heat resistance and high-temperature compression strength, solves the problems of easy cracking and rolling of the pipeline in the cooling stage of continuous winding pipeline production, and perfectly matches the continuous winding molding process of glass fiber reinforced plastic pipeline. DETAILED DESCRIPTION

[0023] The high yield strength continuously wound unsaturated polyester resin and the method for preparing the resin thereof in the present invention will be further described below in conjunction with specific embodiments.

[0024] The preparation method of the high yield strength continuously wound unsaturated polyester resin of the present invention comprises the following steps: S1, adding diol, PET and catalyst into a reaction kettle, introducing nitrogen, stirring, heating to 180°C at 50°C / hour, and then raising the kettle temperature to 220±5°C at 15°C / hour, fully reflux and heat preservation, sampling and testing every 1h, until the sample: propylene glycol monomethyl ether (RX-064) = 1-1.5 is completely clarified after being mixed, and the sample: methanol = 0.5-1.2 is turbid after mixing and starts to cool down, and the temperature drops by 150°C;

[0025] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0026] S3: adding the reactants into the diluent and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0027] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0028] In view of the problem that the resin of the continuous winding pipe has low heat resistance and low compression strength at high temperature, the present invention proposes to introduce crystalline segments into the unsaturated polyester, and utilize crystallization to improve the heat resistance and high temperature compression strength of the resin. PET is a crystalline saturated polyester with good comprehensive performance, excellent physical and mechanical properties in a wide temperature range, long-term use temperature up to 120°C, and high dimensional stability. At present, the recycling of waste PET is mainly through depolymerizing it into monomers and then reusing it as a raw material. The PET depolymerization reaction is divided into three steps: first, it is carried out on the part of the amorphous area connected to the PET crystalline area, and the average molecular weight is reduced to 1 / 3 of the original PET; secondly, it is further depolymerized into oligomers; and finally depolymerized into monomers. The present invention utilizes the alcoholysis method and controls the alcoholysis reaction to proceed only to the second step, introduces the PET crystalline segment into the unsaturated polyester, thereby improving the heat resistance and high temperature compression strength of the resin.

[0029] The present invention will be further described below in conjunction with specific embodiments.

[0030] Example 1

[0031] A continuous winding pipe unsaturated polyester resin with good heat resistance and high high temperature compression strength is made of the following weight ratio:

[0032]

[0033] A method for preparing a continuously wound pipe unsaturated polyester resin having good heat resistance and high high-temperature compression strength, comprising the following steps:

[0034] S1 Add diol, PET polyester chips and catalyst into the reactor, stir, heat up to 180℃ at 50℃ / hour, then raise the reactor temperature to 220±5℃ at 15℃ / hour, fully reflux and keep warm, take samples every 1h for testing, until the sample: RX-064 = 1~1.5 is completely clear after mixing, sample: methanol = 0.5~1.2 is turbid after mixing and starts to cool down, the temperature drops by 150℃;

[0035] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0036] S3: adding the reactants into styrene and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0037] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0038] Example 2

[0039] A continuous winding pipe unsaturated polyester resin with good heat resistance and high high temperature compression strength is made of the following weight ratio:

[0040]

[0041] A method for preparing a continuously wound pipe unsaturated polyester resin having good heat resistance and high high-temperature compression strength, comprising the following steps:

[0042] S1 Add diol, PET bottle flakes and catalyst into the reactor, stir, heat up to 180℃ at 50℃ / hour, then raise the reactor temperature to 220±5℃ at 15℃ / hour, fully reflux and keep warm, take samples every 1h for testing, until the sample: RX-064 = 1~1.5 is completely clear after mixing, sample: methanol = 0.5~1.2 is turbid after mixing and starts to cool down, the temperature drops by 150℃;

[0043] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0044] S3: adding the reactants into styrene and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0045] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0046] Example 3

[0047] A continuous winding pipe unsaturated polyester resin with good heat resistance and high high temperature compression strength is made of the following weight ratio:

[0048]

[0049] A method for preparing a continuously wound pipe unsaturated polyester resin having good heat resistance and high high-temperature compression strength, comprising the following steps:

[0050] S1 Add diol, PET recycled material and catalyst into the reactor, stir, heat up to 180℃ at 50℃ / hour, then heat up to 220±5℃ at 15℃ / hour, fully reflux and keep warm, take samples every 1h for testing, until the sample: RX-064=1~1.5 is completely clear after mixing, the sample: methanol=0.5~1.2 is turbid after mixing and starts to cool down, the temperature drops by 150℃;

[0051] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0052] S3: adding the reactants into styrene and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0053] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0054] Comparative Example 1

[0055] The preparation method of the continuous winding pipe unsaturated polyester resin of this comparative example is substantially the same as that of Examples 1-3, except that phthalic anhydride (PA) is used instead of PET in the raw material of the unsaturated polyester resin of this comparative example.

[0056] The unsaturated polyester resin for the continuous winding pipe of this comparative example is made of the following weight ratio:

[0057]

[0058] The preparation method of the unsaturated polyester resin for continuous winding pipe of this comparative example comprises the following steps:

[0059] S1: Add diol, MA, PA and catalyst into the reactor, stir, and quickly heat up to 205-210°C, control the head temperature at 100±2°C, react at a constant temperature until the acid value reaches 38-44 mgKOH / g, and cool down to 170-180°C;

[0060] S2: adding the reactants into styrene and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0061] S3 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0062] Comparative Example 2

[0063] The preparation method of the continuous winding pipe unsaturated polyester resin in this comparative example is substantially the same as that of Examples 1-3, except that the PET in this comparative example is completely alcoholyzed, and the alcoholysis product is a monomer.

[0064] The unsaturated polyester resin for the continuous winding pipe of this comparative example is made of the following weight ratio:

[0065]

[0066] The preparation method of the unsaturated polyester resin for continuous winding pipe of this comparative example comprises the following steps:

[0067] S1 Add diol, PET polyester chips and catalyst into the reactor, stir, heat up to 180℃ at 50℃ / hour, then raise the reactor temperature to 220±5℃ at 15℃ / hour, fully reflux and keep warm, take samples every 1h for testing, until the sample: methanol = 0.5-1.2 is miscible and completely clarified, start cooling, and the temperature drops by 150℃;

[0068] Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C;

[0069] S3: adding the reactants into styrene and stirring evenly, during which the material temperature is controlled at 70-80°C;

[0070] S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

[0071] Some properties of the unsaturated polyester resins prepared in Examples 1 to 3 are shown in Table 1:

[0072] Table 1: Performance test results of unsaturated polyester resin materials for continuous winding pipes

[0073]

[0074] It can be seen from Examples 1-3 and Comparative Example 1 in Table 1 that Comparative Example 1 is a common orthophthalic FRP pipe resin, and the orthophthalic structure is not crystalline, while Examples 1-3 introduce PET polymers with crystalline segments into the unsaturated polyester resin for continuous winding pipes prepared by the preparation method of the present invention, which are solidified and crystallized, thereby improving the heat resistance of the resin, greatly enhancing the compressive strength and yield strength at high temperatures, and better matching the continuous winding molding process of the FRP pipe.

[0075] It can be seen from Examples 1-3 and Comparative Example 2 in Table 1 that the unsaturated polyester resin material for continuous winding pipes prepared by the preparation method of the present invention in Examples 1-3 introduces PET crystalline segments instead of monomers, thereby improving the heat resistance, compressive strength and yield strength of the resin at high temperatures.

[0076] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent claim scheme. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A high yield strength continuously wound unsaturated polyester resin, characterized in that: Its mass composition is as follows: Maleic anhydride MA 20-25 parts, PET 20-30 parts, 20-25 parts of diol, 25-30 parts of diluent, The catalyst is added in an amount of 0.02-0.06% of the total weight of the unsaturated polyester resin. A polymerization inhibitor added in an amount of 0.01-0.05% of the total weight of the unsaturated polyester resin; The method for preparing the high yield strength continuously wound unsaturated polyester resin comprises the following steps: S1 Add diol, PET and catalyst into the reactor, stir, heat up to 180℃ at 50℃ / hour, then heat up to 220±5℃ at 15℃ / hour, fully reflux and keep warm, take samples every 1h for testing, until the sample: propylene glycol monomethyl ether (RX-064) = 1~1.5 is completely clear after mixing, and the sample: methanol = 0.5~1.2 is turbid after mixing and starts to cool down, and the temperature drops to 150℃; Add MA to S2, raise the kettle temperature to 205-210°C at 15°C / hour, react at constant temperature until the acid value reaches 38-44 mgKOH / g, and cool to 170-180°C; S3: adding the reactants into the diluent and stirring evenly, during which the material temperature is controlled at 70-80°C; S4 is cooled to 35°C and discharged to obtain unsaturated polyester resin.

2. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The molar ratio of maleic anhydride to diol is 1:

1.

3. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The diol package is one or more selected from propylene glycol, ethylene glycol, diethylene glycol, dipropylene glycol, and neopentyl glycol.

4. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The PET is PET polyester chips, PET bottle chips and PET materials recycled in daily life.

5. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The diluent is styrene.

6. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The catalyst is zinc acetate.

7. The high yield strength continuously wound unsaturated polyester resin according to claim 1, characterized in that: The polymerization inhibitor is selected from one of hydroquinone HQ, methyl hydroquinone THQ and p-benzoquinone PBQ.