A kind of high temperature resistant, earthquake resistant and corrosion resistant structural glue and its preparation method and application

By adopting a specific formula of high-temperature, earthquake-resistant and corrosion-resistant structural glue, the existing structural glue has solved the problems of low bond strength and poor corrosion resistance in high temperature and corrosion environments, and achieved the effect of high bond strength and excellent corrosion resistance. Extend the service life of the substrate.

CN115746759BActive Publication Date: 2024-11-29KUNMING UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211530303.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-11-29
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

In high temperature, high pressure and harsh corrosive environments, the existing structural glue has low bond strength, poor wear resistance and corrosion resistance, which can easily lead to cracking and falling off the coating or corrosion damage, affecting the use effect and life.

Method used

High temperature, earthquake-resistant and corrosion-resistant structural glue composed of phenolic resin, polyurethane resin, stearamide, cured corrosion-resistant, flame retardant and leveling agent is used to form high solid content and fast self-curing through specific formulation and preparation processes. Coating to improve bonding strength and corrosion resistance.

Benefits of technology

This structural glue has high bonding strength, extensive material adaptability, excellent corrosion protection performance, good shock resistance, wear resistance, water resistance and heat resistance, which can extend the service life of the substrate and reduce the high-temperature airflow to the heated surface Wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746759B_ABST
    Figure CN115746759B_ABST
Patent Text Reader

Abstract

The invention discloses a high temperature resistant, earthquake resistant and anti-corrosion structural glue and its preparation method and application. The structural glue is composed of the following raw materials in parts by weight: 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 21-25 parts of curing anti-corrosion agent, 11-15 parts of flame retardant, and 9-11 parts of leveling agent. The high temperature resistant, earthquake resistant and anti-corrosion coating can have a long shelf life, convenient construction, strong and durable, and high bonding strength, a wide range of bonding materials, water resistance, high corrosion resistance, high alkali resistance, high hardness, high temperature resistance. The high temperature resistant, earthquake resistant and anti-corrosion structural glue of the present invention has a simple preparation process, is an ideal anti-corrosion coating, and is worthy of industrial promotion. Its temperature resistance can reach more than 100°C, is not easy to melt, and better reduces the wear of the high temperature airflow on the heated surface, reduces the high temperature corrosion rate, and prolongs the service life of the substrate, which is conducive to practical use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of structural adhesives, and specifically relates to high temperature resistant, shock resistant and corrosion resistant structural adhesive and a preparation method and application thereof. Background Art

[0002] In industrial furnaces and thermal equipment, structural glue is needed to bond the substrate for industrial furnace applications. Structural glue is applied between two objects. When the water in the glue disappears, the polymer in the glue relies on the mutual tension to tightly bind the two objects together to play a bonding role. The bonding of objects is achieved by the tension between the polymers in the glue. However, since the furnace body and pipelines are in a high-temperature environment, and the high-temperature gas contains sulfides, chlorides and sulfates, the bonding force is reduced by the temperature, causing it to fall off, and the usability is significantly limited, and it will cause serious corrosion to them. In order to reduce the wear and corrosion between equipment, by coating the heated part with high-temperature and corrosion-resistant structural glue, while playing a bonding role, it serves as a protective layer for the equipment, reducing the wear of the high-temperature airflow on the equipment, reducing the high-temperature corrosion rate, and extending the service life of the furnace body, pipelines and thermal equipment.

[0003] The structural adhesives currently sold on the market have low bonding strength with the base material and poor wear resistance and corrosion resistance in harsh environments of high temperature, high pressure and corrosion, which can easily cause cracking or corrosion damage to the coating during use, thus affecting the use effect and service life. On the other hand, the physical and chemical properties of the heating surface pipe materials and refractory materials directly affect the safety, energy saving, production capacity and environmental protection performance of industrial furnaces.

[0004] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention

[0005] The first purpose of the present invention is to provide a high temperature resistant, shock resistant and corrosion resistant structural glue. The second purpose of the present invention is to provide a preparation method of the high temperature resistant, shock resistant and corrosion resistant structural glue. The third purpose of the present invention is to provide an application of the high temperature resistant, shock resistant and corrosion resistant structural glue.

[0006] The first object of the present invention is achieved by providing a high temperature resistant, shock resistant and corrosion resistant structural adhesive, which is composed of the following raw materials in parts by weight:

[0007] 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 21-25 parts of curing anti-corrosion agent, 11-15 parts of flame retardant, and 9-11 parts of leveling agent.

[0008] The second object of the present invention is achieved by the method for preparing the high temperature resistant, shock resistant and corrosion resistant structural adhesive according to the following steps:

[0009] S1, placing phenolic resin and polyurethane resin in a reaction kettle according to the formula parts and stirring them first, then weighing stearamide according to the formula parts and pouring it into the reaction kettle, heating and stirring, to obtain a mixture A;

[0010] S2, when the temperature inside the reactor reaches a certain temperature, add flame retardant and leveling agent into the reactor according to the formula, and add them into mixture A; after continuous heating, add curing anti-corrosion agent into the reactor according to the formula, and obtain mixture B after stirring;

[0011] S3. Add deionized water to the obtained mixture B, and slowly cool it to obtain the target high temperature resistant, shock resistant and corrosion resistant structural adhesive.

[0012] The curing anticorrosive agent is prepared by the following steps:

[0013] a. Add metal silicate and deionized water into a reactor, introduce nitrogen to replace the air, protect the reaction in the reactor, stir at a certain speed and temperature, and cool to room temperature to obtain intermediate I;

[0014] b. Add the intermediate I and hydrochloric acid into a reaction kettle, stir until completely mixed under a certain speed and temperature, and then react to obtain a curing anticorrosive agent. The reaction formula is as follows:

[0015] Na2SiO3+2HCl=2NaCl+H2SiO3.

[0016] The third object of the present invention is achieved by using the high temperature resistant, shock resistant and corrosion resistant structural glue as an adhesive between the same or different substrates.

[0017] The present invention has the following beneficial effects:

[0018] 1. The high temperature resistant, earthquake resistant and corrosion resistant structural glue provided by the present invention can be stored for up to 26 months. Compared with existing products on the market, the stirring time and curing time are greatly shortened. The solid content is higher than that of existing glue products. After combining silicate and hydrochloric acid, the two can be quickly self-cured to form a hard thick film coating, so that the formed coating has excellent corrosion protection performance, high earthquake resistance, wear resistance, water resistance and heat resistance, can be machined, is easy to construct and is strong and durable, and further improves the coating performance.

[0019] 2. This structural glue has high bonding strength and a wide range of bonding materials. It can be used for bonding the same or different materials such as metals, plastics, and ceramics. It can partially replace traditional connection forms such as welding and riveting. Therefore, it has a high hardness and can be tightly combined with the substrate to form a dense protective layer. In addition, its temperature resistance can reach above 100°C and is not easy to melt. It can effectively reduce the wear of the heated surface by high-temperature airflow, reduce the high-temperature corrosion rate, extend the service life of the substrate, and is conducive to practical use. Specific parameters are shown in Table 1.

[0020] Table 1 Main process parameters of high temperature resistant, earthquake resistant and corrosion resistant structural glue according to Example 1 of the present invention

[0021] BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the sample picture before the salt spray test of Test Example 1;

[0023] Figure 2 This is the sample picture after the salt spray test of Test Example 1. DETAILED DESCRIPTION

[0024] The technical features, purposes and beneficial effects of the present invention will be more clearly understood in conjunction with specific embodiments below. The technical solution of the present invention is now described in detail below, but it should not be construed as limiting the scope of implementation of the present invention.

[0025] The invention provides a high temperature resistant, shock resistant and corrosion resistant structural glue, which is composed of the following raw materials in parts by weight: 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 21-25 parts of curing anti-corrosion agent, 11-15 parts of flame retardant and 9-11 parts of leveling agent.

[0026] The flame retardant is magnesium hydroxide, aluminum hydroxide or glass fiber.

[0027] The leveling agent is polyterephthalic acid or polydimethylsiloxane.

[0028] The preparation process of the high temperature resistant, shock resistant and corrosion resistant structural glue is as follows:

[0029] S1, placing phenolic resin and polyurethane resin in a reaction kettle according to the formula parts and stirring them first, then weighing stearamide according to the formula parts and pouring it into the reaction kettle, heating and stirring, to obtain a mixture A;

[0030] S2, when the temperature inside the reactor reaches a certain temperature, add flame retardant and leveling agent into the reactor according to the formula, and add them into mixture A; after continuous heating, add curing anti-corrosion agent into the reactor according to the formula, and obtain mixture B after stirring;

[0031] S3. Add deionized water to the obtained mixture B, and slowly cool it to obtain the target high temperature resistant, shock resistant and corrosion resistant structural adhesive.

[0032] The curing anticorrosive agent is prepared by the following steps:

[0033] a. Add metal silicate and deionized water into a reactor, introduce nitrogen to replace the air, protect the reaction in the reactor, stir at a certain speed and temperature, and cool to room temperature to obtain intermediate I;

[0034] b. Add the intermediate I and hydrochloric acid into a reaction kettle, stir until completely mixed under a certain speed and temperature, and then react to obtain a curing anticorrosive agent. The reaction formula is as follows:

[0035] Na2SiO3+2HCl=2NaCl+H2SiO3.

[0036] In step S1, the internal heating temperature of the reactor is set to 70° C., the stirring speed is 2500 r / min, and the stirring time is 25 minutes.

[0037] In step S2, the internal heating temperature of the reactor is set to 80° C., and then continued to be heated to 150° C., the stirring speed is 5000 r / min, and the stirring time is 45 minutes.

[0038] In the step a, the molar ratio of sodium oxide to metal oxide in the metal silicate is 5.3:1-5.6:1, the internal temperature of the reactor is 125° C.-130° C., the stirring speed is 5000-6000 r / min, and the stirring time is 20-30 minutes.

[0039] In the step b, the internal temperature of the reactor is 70°C-85°C, the stirring speed is 1500-2000 r / min, and the reaction time is 2-3 hours.

[0040] The present invention also provides an application of the high temperature resistant, shock resistant and corrosion resistant structural glue, which is used as an adhesive between the same or different substrates.

[0041] The substrate is metal, plastic or ceramic

[0042] Example 1

[0043] A high temperature resistant, shock resistant and corrosion resistant structural glue is prepared from the following raw materials in parts by weight:

[0044] 25 parts of phenolic resin, 18 parts of polyurethane resin, 16 parts of stearamide, 25 parts of curing anti-corrosion agent, 11 parts of flame retardant, and 9 parts of leveling agent.

[0045] The preparation method of the high temperature resistant, shock resistant and corrosion resistant structural adhesive comprises the following steps:

[0046] S1. Phenolic resin and polyurethane resin are placed in a reactor according to the formula and stirred first, then stearamide is weighed according to the formula and poured into the reactor, heated to 70° C., stirred at a speed of 2500 r / min, and stirred for 25 minutes to obtain a mixture A;

[0047] S2. When the temperature inside the reactor reaches 80°C, add flame retardant and leveling agent into the reactor according to the formula, and add them into mixture A. Continue heating to 150°C, add curing anti-corrosion agent into the reactor according to the formula, stir at a speed of 5000 r / min, stir for 45 minutes, and obtain mixture B after stirring.

[0048] S3. Add deionized water to the obtained mixture B and slowly cool it at a temperature of 22-25° C. for 2 hours until it is completely cured to obtain a high temperature resistant, shock resistant and corrosion resistant structural glue.

[0049] The curing anticorrosive agent is prepared by the following steps:

[0050] Step A: Add metal silicate and deionized water into a reactor, introduce nitrogen to replace the air, and protect the reaction in the reactor. Stir for 25 minutes at a speed of 5300 r / min and a temperature of 125°C, and then cool to room temperature to obtain intermediate 1;

[0051] Step B: Add intermediate 1 and hydrochloric acid into a reactor, stir until completely mixed at a speed of 1800 r / min and a temperature of 75°C, and react for 2 hours to obtain the following reaction formula:

[0052] Na2SiO3+2HCl=2NaCl+H2SiO3

[0053] Example 2

[0054] A high temperature resistant, shock resistant and corrosion resistant structural glue is prepared from the following raw materials in parts by weight:

[0055] 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 24 parts of curing anti-corrosion agent, 11-15 parts of flame retardant, and 9-11 parts of leveling agent.

[0056] The preparation method of the high temperature resistant, shock resistant and corrosion resistant structural adhesive comprises the following steps:

[0057] S1: Phenolic resin and polyurethane resin are placed in a reactor according to the formula and stirred first, then stearamide is weighed according to the formula and poured into the reactor, heated to 70°C, stirred at a speed of 2500 r / min, and stirred for 25 minutes to obtain a mixture A;

[0058] S2: When the temperature inside the reactor reaches 80°C, add flame retardant and leveling agent into the reactor according to the formula, and add them into mixture A. Continue heating to 150°C, add curing anti-corrosion agent into the reactor according to the formula, stir at a speed of 5000 r / min, stir for 45 minutes, and obtain mixture B after stirring;

[0059] S3: Add deionized water to the obtained mixture B, and slowly cool it at a temperature of 22-25° C. for 2 hours until it is completely cured, thereby obtaining a high temperature resistant, shock resistant, and corrosion resistant structural adhesive.

[0060] The curing anticorrosive agent is prepared by the following steps:

[0061] a. Add metal silicate and deionized water into a reactor, introduce nitrogen to replace the air, and protect the reaction in the reactor. Stir for 30 minutes at a speed of 5800 r / min and a temperature of 125°C, and then cool to room temperature to obtain intermediate 1;

[0062] b. Add intermediate 1 and hydrochloric acid into a reactor, stir until completely mixed at a speed of 2000 r / min and a temperature of 80°C, and react for 3 hours to obtain a cured anticorrosive agent. The reaction formula is as follows:

[0063] Na2SiO3+2HCl=2NaCl+H2SiO3

[0064] Test Example 1

[0065] The high temperature resistant, shock resistant and anti-corrosion structural glue obtained in Example 1 was subjected to a salt spray test, i.e., an anti-corrosion test. The salt spray test is an environmental test to verify the corrosion resistance of materials under simulated salt spray environmental conditions. The corrosion components of oxygen, carbon dioxide and chloride (the product brought by the ocean and inland saline-alkali areas such as sodium chloride in the atmospheric flow process) in the salt spray environment are used to cause the material to deteriorate or be damaged. The corrosion mechanism of salt spray on the surface of metal materials is that water vapor condenses and aggregates on the metal surface, and the chloride ions therein destroy and pass through the oxide layer on the metal surface to react electrochemically with the internal metal. At the same time, chloride ions containing a certain hydration energy are easily adsorbed in the pores and cracks on the metal surface, replacing the oxygen in the oxide layer, turning the originally insoluble oxide into a soluble chloride, and turning the passive surface of the metal into an active surface, thereby causing corrosion damage to the metal. The salt spray test box used is a test equipment with a certain volume space, and a salt spray environment is created in its volume space to assess the quality of the material's salt spray corrosion resistance. Compared with the natural environment, the chloride concentration in the salt spray environment inside the equipment is several times or even dozens of times higher than the chloride content in the general natural environment. In this environment, the corrosion rate of metals is greatly increased, so the time required for salt spray testing of materials is also reduced accordingly, thereby improving the test efficiency. If a material sample is tested in a natural exposure environment, it may take a year or even longer to achieve the desired results, while in a salt spray environment, similar results can be obtained in just tens of hours or even hours. Take three iron plates and label them No. 1-3. Among them, No. 1 is a pure iron plate, No. 2 is a high-temperature resistant, shock-resistant, and corrosion-resistant structural glue prepared in Example 1 that is applied on the steel instead of welding, and No. 3 is a commercially available product without a curing anti-corrosion agent prepared in Comparative Example 1 that is applied on the iron plate instead of welding. Figure 1 Put No. 1-3 into the salt spray test chamber, and after 72 hours, Figure 2 The corrosion rate v is calculated according to the following formula, and the test results are shown in Table 2:

[0066]

[0067] Where V: Corrosion weight loss per unit area, g / m 2 ·h;

[0068] W1: initial mass of sample, g;

[0069] W2: The mass of the sample after the corrosion product is removed after the corrosion test, g;

[0070] S: sample surface area, m 2 ;

[0071] t: Salt spray test time, h.

[0072] Table 2 Salt spray test results

[0073] Sample Type Original (g) Weight loss (g) <![CDATA[Area (m 2 )]]> <![CDATA[Corrosion rate (g / m 2 ·h)]]> Pure iron plate (No. 1) 57.607 0.524 0.0075 1.456 This research glue (No. 2) 85.839 0.066 0.0075 0.183 Commercially available product without curing anticorrosive agent (No. 3) 73.312 0.162 0.0075 0.450

[0074] As shown in Table 2, the corrosion resistance of pure iron plate is the worst, with a corrosion rate of 1.456 g / m 2 h, the high temperature anti-seismic and anti-corrosion structural adhesive prepared in Example 1 has the best corrosion resistance, with a corrosion rate of 0.183 g / m 2 ·h.

[0075] This salt spray test is combined with a 72-hour test. The Zn(OH)2 or ZnCl2·4Zn(OH)2 generated by corrosion will hydrolyze into ZnO. The presence of ZnO in high-temperature, shock-resistant and corrosion-resistant structural glue will inhibit its generation and improve the adhesion and density of the corrosion products, thereby forming a corrosion product protective film on the corrosion surface with strong adhesion, firmness, density and good insulation.

[0076] Test Example 2

[0077] The high temperature resistant, shock resistant and corrosion resistant structural glue (1 # ) and HFVC anti-corrosion structural adhesive (2 # ), the performance ratio test was carried out under the condition of muffle furnace at 300℃. # Instead of welding, the coating is adhered to the steel to improve the hardness of the steel. The preparation process parameters of the two are shown in Table 3.

[0078] Table 3 Main process parameters of the high temperature resistant, earthquake resistant and corrosion resistant structural adhesive and HFVC corrosion resistant structural adhesive of the present invention

[0079] performance <![CDATA[1 # Parameters]]> <![CDATA[2 # Parameters]]> volatility none none Stirring time (min) 25-45 120 Cooling time (h) 4-6 24-72 Working temperature(℃) -50-400 -50-100 Retention time (month) ≥ 26 6

[0080] Result: with 2 # In comparison, 1 # The performance is not affected by the high temperature environment, no cracks or gaps appear, it does not melt or fall off, it can still be used, and the wear is small.

Claims

1. A high temperature resistant, shock resistant and corrosion resistant structural glue, characterized in that: The high temperature resistant, shock resistant and corrosion resistant structural glue is made of 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 21-25 parts of curing anticorrosion agent, 11-15 parts of flame retardant and 9-11 parts of leveling agent measured by weight; the curing anticorrosion agent is prepared by the following steps: a. Sodium silicate and deionized water were added into a reactor, nitrogen was introduced to replace the air to protect the reaction in the reactor, and the mixture was stirred at a speed of 5000-6000 r / min and 125° C.-130° C. for 20-30 min, and then cooled to room temperature to obtain intermediate I; b. Add intermediate I and hydrochloric acid into a reactor, stir until completely mixed at a speed of 1500-2000 r / min and 70°C-85°C, and react for 2-3 hours to obtain a curing anticorrosive agent, and the reaction formula is Na2SiO3+2HCl=2NaCl+H2SiO3; The high temperature resistant, shock resistant and corrosion resistant structural adhesive is prepared according to the following steps: S1. Phenolic resin and polyurethane resin are placed in a reactor according to the number of parts in the formula and stirred first, then stearamide is weighed according to the number of parts in the formula and poured into the reactor, heated to 70° C., and stirred at a stirring speed of 2500 r / min for 25 min to obtain a mixture A; S2. When the temperature inside the reactor reaches 80°C, add flame retardant and leveling agent into the reactor according to the formula, and add them into mixture A; after continuously heating to 150°C, add curing anti-corrosion agent into the reactor according to the formula, and stir at a stirring speed of 5000r / min for 45min to obtain mixture B; S3. Add deionized water to the obtained mixture B and slowly cool it down at a temperature of 22-25° C. for 2 hours until it is completely cured, thereby obtaining the target high temperature resistant, shock resistant and corrosion resistant structural glue.

2. The high temperature resistant, shock resistant and corrosion resistant structural glue according to claim 1, characterized in that: The flame retardant is magnesium hydroxide or aluminum hydroxide.

3. The high temperature resistant, shock resistant and corrosion resistant structural glue according to claim 1, characterized in that: The leveling agent is polydimethylsiloxane.

4. Use of the high temperature resistant, shock resistant and corrosion resistant structural adhesive according to claim 1, 2 or 3 as an adhesive between the same or different substrates.

5. The use according to claim 4, characterized in that: The substrate is metal, plastic or ceramic.

Citation Information

Patent Citations

  • A method for preparing a phenolic resin-polyurethane adhesive

    CN102295909A

  • Organic / inorganic hybridization-modified phenolic resin for aluminum carbon refractory material and preparation method thereof

    CN104109223A

  • Preparing method of antioxidant high-temperature-resistant phenolic resin binder

    CN107756270A

  • urea-formaldehyde resins AND PROCESS FOR THEIR MANUFACTURE

    DE2642450A1