Two-component polyurethane adhesive and preparation method thereof
By using two-component polyurethane glue with components such as modified polyol and prepolymer in aluminum alloy and glass assembly, the problem of inability to be easily disassembled and reworked in the existing technology is solved, and high-strength, fast bonding and convenient rework are achieved. The effect is to reduce the scrap rate and production costs.
Patent Information
- Application Number
- CN202211541310.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-01
AI Technical Summary
The existing two-component polyurethane adhesive cannot be easily disassembled and reworked when errors occur in the assembly of aluminum alloy and glass, resulting in high scrap rates and production costs.
A two-component polyurethane glue is used that includes a resin component and a curing agent component. The resin component is composed of modified polyol, catalyst, plasticizer and powder. The curing agent component is composed of prepolymer, plasticizer, powder. It is composed of body and water remover. Through specific formula and preparation method, it can achieve high strength and rapid bonding and facilitate rework.
While achieving high strength and fast bonding, it can be easily reworked at 60°C, reducing the scrap rate and optimizing production costs.
Smart Images

Figure BDA0003976000820000071 
Figure BDA0003976000820000081 
Figure BDA0003976000820000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a two-component polyurethane adhesive and a preparation method thereof. Background Art
[0002] At present, the two-component polyurethane adhesive used for bonding aluminum alloy and glass can achieve high strength and fast bonding by using conventional raw materials and adding catalysts. However, when errors or large errors occur in the assembly of aluminum alloy and glass, rework is required. However, based on the high-strength and fast bonding characteristics of the existing two-component polyurethane, the aluminum alloy and glass after bonding cannot be separated for rework, resulting in a high scrap rate and increased production costs.
[0003] In view of this, it is necessary to propose an adhesive that has both high strength and fast bonding properties and is easy to rework. Summary of the invention
[0004] The purpose of the present invention is to provide a two-component polyurethane adhesive and a preparation method thereof. The two-component polyurethane adhesive has the characteristics of high bonding strength, rapid bonding and easy rework, and the preparation method has simple steps and is easy to operate.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] A two-component polyurethane adhesive comprises a resin component and a curing agent component;
[0007] The resin component includes polyol, catalyst, plasticizer and powder;
[0008] The curing agent components include prepolymer, plasticizer, powder and dehydrating agent;
[0009] The polyol is selected from one or more of polyether polyol, modified castor oil polyol, modified soybean oil polyol or modified palm oil polyol;
[0010] The prepolymer is an NCO-terminated prepolymer obtained by reacting one or more of PAPI, MDI, TDI, HMDI, HDI trimer, IPDI and polyol.
[0011] Furthermore, the resin component comprises, by mass percentage, 30-60% of polyol, 0-20% of plasticizer, 0-0.1% of catalyst, and 30-60% of powder;
[0012] In terms of mass percentage, the curing agent component comprises 40-60% of prepolymer, 0-10% of plasticizer, 30-50% of powder, and 0.1-1.0% of dehydrating agent.
[0013] Furthermore, the polyol used in the prepolymer is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000;
[0014] The mass content of NCO in the NCO-terminated prepolymer is 1-9%.
[0015] Furthermore, the polyether polyol in the resin component is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000;
[0016] The molecular weight of the bifunctional polyether polyol is 1000-2000; the molecular weight of the trifunctional polyether polyol is 3000-5000.
[0017] Furthermore, the powder in the resin component is selected from one or more of gas silica, heavy calcium, modified nano calcium, calcined kaolin, carbon black, and molecular sieve activated powder;
[0018] The powder in the curing agent component is selected from two or more of gas silica, silica powder, heavy calcium, nano calcium, modified nano calcium, calcined kaolin, talc and carbon black.
[0019] Furthermore, the catalyst is one or more of stannous octoate, dibutyltin dilaurate, bismuth isooctanoate and zinc isooctanoate.
[0020] Furthermore, the plasticizers in the resin component and the curing agent component are one or more of DBP, DOP, DINP, DOA, DOTP, and TXIP.
[0021] Furthermore, the dehydrating agent is p-toluenesulfonyl isocyanate.
[0022] A method for preparing a two-component polyurethane adhesive, the method is used to prepare the above-mentioned two-component polyurethane adhesive; the method comprises the following steps:
[0023] Preparation of resin component: pre-dehydrate all raw materials at high temperature, add other raw materials except catalyst into planetary stirring kettle, stir evenly at room temperature, maintain vacuum for 30-60 minutes, add catalyst after breaking vacuum, continue stirring and dispersing under vacuum for 10-20 minutes, and obtain the resin component;
[0024] Preparation of curing agent component: Prepolymer, plasticizer and powder are dispersed evenly in a planetary stirring kettle and vacuum is maintained for 30-60 minutes. After breaking the vacuum, dehydrating agent is added and stirring and dispersing is continued for 10-20 minutes under vacuum to obtain the resin component.
[0025] Furthermore, the preparation method of the prepolymer is: vacuuming and removing water from the polyol at 120° C. for 1.5-2 hours, cooling to 80-90° C. and breaking the vacuum, then adding one or more of PAPI, MDI, TDI, HMDI, HDI trimer, and IPDI, and keeping the temperature for reaction for 2-4 hours. After the NCO mass content of the test reactant reaches 1-9%, cooling and removing bubbles are performed to obtain the NCO-terminated prepolymer.
[0026] The technical solution provided by the present invention may include the following beneficial effects:
[0027] The present invention modifies the vegetable oil polyol with polyester polyol or a small molecular weight chain extension crosslinking agent, adds a group with good bonding effect on aluminum alloy / glass, and fully utilizes the advantages of good toughness of long carbon chain and high strength of modifier to achieve the above purpose. The polyol in the resin component of the invention adopts polyether polyol, modified castor oil polyol, modified soybean oil polyol and / or modified palm oil polyol, wherein the modified vegetable oil polyol can enhance the bonding strength between polyurethane adhesive and aluminum alloy to achieve the effect of fast bonding and high strength, and retains the toughness of vegetable oil polyol, which is convenient for subsequent rework of polyurethane adhesive construction.
[0028] Based on the formula setting of the resin component and the curing agent component of the present invention, the present invention can achieve the effect of rapid high bonding strength and rapid rework at 60° C. without residual adhesive on aluminum alloy and glass by adding a small amount of catalyst. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further explained below in conjunction with specific implementation methods.
[0030] The present invention provides a two-component polyurethane adhesive, comprising a resin component and a curing agent component;
[0031] The resin component includes polyol, catalyst, plasticizer and powder;
[0032] The curing agent components include prepolymer, plasticizer, powder and dehydrating agent;
[0033] The polyol is selected from one or more of polyether polyol, modified castor oil polyol, modified soybean oil polyol or modified palm oil polyol;
[0034] The prepolymer is an NCO-terminated prepolymer obtained by reacting one or more of PAPI, MDI, TDI, HMDI, HDI trimer, IPDI and polyol.
[0035] The two-component polyurethane adhesive of the present invention is used for bonding aluminum alloy to glass, and is also suitable for bonding other materials with relatively large polarity, such as bonding between rubber materials and metal materials, and bonding between stainless steel, copper or titanium alloy and glass.
[0036] PAPI is polymethylene polyphenyl polyisocyanate, MDI is diphenylmethane-4,4'-diisocyanate, TDI is 2,4-diisocyanato-1-methylbenzene, HMDI is 4,4'-dicyclohexylmethane diisocyanate, HDI trimer is the trimer of hexamethylene diisocyanate, and IPDI is isophorone diisocyanate. The present invention modifies the vegetable oil polyol with polyester polyol or a small molecular weight chain extension crosslinking agent, adds a group with good bonding effect on aluminum alloy / glass, and fully utilizes the advantages of good toughness of long carbon chain and high strength of modifier to achieve the above purpose.
[0037] Vegetable oil polyols are widely used in polyurethane adhesives due to their low price, wide sources and good toughness, but their bonding effect on metals such as aluminum alloys is poor. Compared with petroleum-based polyols, they have the advantage of being easy to modify. The polyols in the resin component of the present invention are polyether polyols, modified castor oil polyols, modified soybean oil polyols and / or modified palm oil polyols, wherein the modified vegetable oil polyols can enhance the bonding strength between polyurethane adhesive and aluminum alloy to achieve the effect of rapid bonding and high strength, and retain the toughness of the vegetable oil polyols, which is convenient for subsequent rework of polyurethane adhesive construction.
[0038] Specifically, the modified vegetable oil polyol is polyester-modified castor oil, trimethylolpropane-modified castor oil, polyester-modified soybean oil polyol, trimethylolpropane-modified soybean oil polyol, polyester-modified palm oil polyol, and trimethylolpropane-modified palm oil polyol, wherein polyester modification refers to modifying vegetable oil polyol with polyester polyol. The present invention uses a small molecule chain extender crosslinking agent or a low molecular weight polyester polyol to perform alcoholysis modification on vegetable oil polyol to obtain a polyol containing a polar group, thereby enhancing the bonding strength with aluminum alloy and retaining the toughness of the vegetable oil polyol.
[0039] Preferably, the polyol in the resin component is selected from one or more of modified castor oil polyol, modified soybean oil polyol or modified palm oil polyol and mixed with polyether polyol.
[0040] Furthermore, in terms of mass percentage, the resin component includes 30-60% polyol, 0-20% plasticizer, 0-0.1% catalyst, and 30-60% powder; in terms of mass percentage, the curing agent component includes 40-60% prepolymer, 0-10% plasticizer, 30-50% powder, and 0.1-1.0% dehydrating agent.
[0041] Based on the formula setting of the resin component and the curing agent component of the present invention, the present invention can achieve the effect of high rapid bonding strength by adding a small amount of catalyst, and rapid rework at 60°C, and no residual adhesive on aluminum alloy and glass. Preferably, in terms of mass percentage, the resin component includes 30-50% of polyol, 2-10% of plasticizer, 0.02-0.05% of catalyst, and 45-60% of powder; in terms of mass percentage, the curing agent component includes 45-55% of prepolymer, 2-7% of plasticizer, 40-50% of powder, and 0.3-0.7% of dehydrating agent.
[0042] Specifically, the polyol used in the prepolymer is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000; the mass content of NCO in the NCO-terminated prepolymer is 1-9%. The polyether polyol in the resin component is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000.
[0043] The molecular weights of the polyether polyols in the prepolymer and the resin components are as follows: the molecular weight of the difunctional polyether polyol is 1000-2000; the molecular weight of the trifunctional polyether polyol is 3000-5000.
[0044] Further, the powder in the resin component is selected from one or more of aerosil, heavy calcium, modified nano calcium, calcined kaolin, carbon black, and molecular sieve activated powder; the powder in the curing agent component is selected from two or more of aerosil, silica powder, heavy calcium, nano calcium, modified nano calcium, calcined kaolin, talcum powder, and carbon black; and the powder in the curing agent component is selected from two or more of aerosil, modified nano calcium, and carbon black. The aerosil is also called fumed white carbon black.
[0045] Further, the catalyst is one or more of stannous octoate, dibutyltin dilaurate, bismuth isooctanoate and zinc isooctanoate. The plasticizers in the resin component and the curing agent component are one or more of DBP, DOP, DINP, DOA, DOTP and TXIP. Preferably, the catalyst is dibutyltin dilaurate and the plasticizer is DOTP. The dewatering agent is p-toluenesulfonyl isocyanate.
[0046] Accordingly, the present invention also provides a method for preparing a two-component polyurethane adhesive, which is used to prepare the above-mentioned two-component polyurethane adhesive; the method comprises the following steps:
[0047] Preparation of resin component: pre-dehydrate all raw materials at high temperature, add other raw materials except catalyst into planetary stirring kettle, stir evenly at room temperature, maintain vacuum for 30-60 minutes, add catalyst after breaking vacuum, continue stirring and dispersing under vacuum for 10-20 minutes, and obtain the resin component;
[0048] Preparation of curing agent component: Prepolymer, plasticizer and powder are dispersed evenly in a planetary stirring kettle and vacuum is maintained for 30-60 minutes. After breaking the vacuum, dehydrating agent is added and stirring and dispersing is continued for 10-20 minutes under vacuum to obtain the resin component.
[0049] The preparation method has simple steps and is easy to operate, and can efficiently obtain the high-strength, fast-bonding and easy-rework two-component polyurethane adhesive of the present invention.
[0050] Further, the preparation method of the prepolymer is as follows: the polyol is vacuumed and dehydrated at 120°C for 1.5-2h, the temperature is lowered to 80-90°C and then the vacuum is broken, and then one or more of PAPI, MDI, TDI, HMDI, HDI trimer, and IPDI are added, and the reaction is kept warm for 2-4h. After the NCO mass content of the test reactant reaches 1-9%, the temperature is lowered and the foam is removed to obtain the NCO-terminated prepolymer.
[0051] The present invention is further described below by way of examples and comparative examples.
[0052] Example 1
[0053] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0054]
[0055] Example 2
[0056] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0057]
[0058] Example 3
[0059] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0060]
[0061] Example 4
[0062] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0063]
[0064] Example 5
[0065] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0066]
[0067] Example 6
[0068] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0069]
[0070] Example 7
[0071] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0072]
[0073] Example 8
[0074] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0075]
[0076] Example 9
[0077] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0078]
[0079] Example 10
[0080] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0081]
[0082] Embodiment 11
[0083] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0084]
[0085] Example 12
[0086] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0087]
[0088] Embodiment 13
[0089] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0090]
[0091] Embodiment 14
[0092] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this embodiment in terms of mass percentage is shown in the following table:
[0093]
[0094] Comparative Example 1
[0095] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this comparative example in terms of mass percentage is shown in the following table:
[0096]
[0097] Comparative Example 2
[0098] The formula of the resin component and the curing agent component in the two-component polyurethane adhesive of this comparative example in terms of mass percentage is shown in the following table:
[0099]
[0100] The two-component polyurethane adhesives of Examples 1-14 and Comparative Examples 1-2 were prepared by the following method, as follows:
[0101] Preparation of resin components: All raw materials are dehydrated at high temperature in advance to make the water content of liquid material less than 500ppm and the water content of powder less than 1000ppm; add other raw materials except catalyst into the planetary stirring kettle, disperse and stir evenly at room temperature and high speed, and keep vacuuming for 30-60 minutes, then break the vacuum, quickly add catalyst, continue vacuuming, stirring and dispersing for 10-20 minutes, and then press the material to produce glue;
[0102] Preparation of curing agent component: dehydrate the plasticizer and powder at high temperature in advance, the moisture content of the plasticizer is less than 500ppm, and the moisture content of the powder is less than 1000ppm; add the prepolymer, plasticizer and powder into the planetary stirring kettle, stir and disperse them evenly at high speed and keep vacuuming for 30-60 minutes, then break the vacuum, quickly add the dehydrating agent, continue vacuuming, stirring and dispersing for 10-20 minutes, and then press the material out of the glue.
[0103] The preparation process of the prepolymer in the curing agent component is: after vacuuming and removing water from the polyol at 120°C for 1.5-2h, cool it down to 80-90°C to break the vacuum, add one or more of PAPI, MDI, TDI, HMDI, HDI trimer, and IPDI, and keep the temperature for 2-4h to measure the NCO mass content. When it meets the requirements, cool it down, evacuate the air to remove bubbles, and then pack it out of the kettle.
[0104] The two-component polyurethane adhesives of Examples 1-14 and Comparative Examples 1-2 were tested, and the test results are shown in the following table.
[0105]
[0106] In the above table, the operable time refers to the time that construction can be carried out after the resin component and the curing agent component are evenly mixed. The two-component polyurethane adhesive must be applied to the bonding area and the two materials must be connected within this time range. The shear strength and 60℃ rework data in the above test results are obtained by bonding aluminum alloy and glass. 60℃ rework means that when rework is required, the two-component polyurethane adhesive at the bonding area is heated to 60℃ and then torn off.
[0107] As can be seen from the above table, the two-component polyurethane adhesives of Examples 1-14 of the present invention all have the characteristics of high strength, fast bonding and easy rework. The resin component of Comparative Example 1 uses aromatic polyester polyols, which leads to sticking phenomenon when reworked at 60°C. This is because aromatic polyester polyols have high polarity, high strength, and high softening point temperature, and cannot be reworked at 60°C. The resin component of Comparative Example 2 uses castor oil polyols. Castor oil polyols have good flexibility due to their long carbon chain, but their strength is worse than that of polyester polyols, and the strength of the glue made is low.
[0108] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A two-component polyurethane adhesive, characterized in that: comprising a resin component and a curing agent component; The resin component includes polyol, catalyst, plasticizer and powder; The curing agent components include prepolymer, plasticizer, powder and dehydrating agent; The polyol is a mixture of one or more of polyester-modified castor oil, trimethylolpropane-modified castor oil, polyester-modified soybean oil polyol, trimethylolpropane-modified soybean oil polyol, polyester-modified palm oil polyol and trimethylolpropane-modified palm oil polyol with polyether polyol; The polyether polyol in the resin component is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000; The molecular weight of the bifunctional polyether polyol is 1000-2000; the molecular weight of the trifunctional polyether polyol is 3000-5000; The prepolymer is an NCO-terminated prepolymer obtained by reacting one or more of PAPI, MDI, TDI, HMDI, HDI trimer, IPDI and a polyol; The polyol used in the prepolymer is a difunctional or trifunctional polyether polyol with a molecular weight of 1000-5000; The mass content of NCO in the NCO-terminated prepolymer is 1-9%.
2. The two-component polyurethane adhesive according to claim 1, characterized in that: In terms of mass percentage, the resin component includes 30-60% polyol, 0-20% plasticizer, 0-0.1% catalyst, and 30-60% powder; In terms of mass percentage, the curing agent component includes 40-60% prepolymer, 0-10% plasticizer, 30-50% powder, and 0.1-1.0% dehydrating agent.
3. The two-component polyurethane adhesive according to claim 1, characterized in that: The powder in the resin component is selected from one or more of gas silica, heavy calcium, modified nano calcium, calcined kaolin, carbon black, and molecular sieve activated powder; The powder in the curing agent component is selected from two or more of gas silica, silica powder, heavy calcium, nano calcium, modified nano calcium, calcined kaolin, talc and carbon black.
4. The two-component polyurethane adhesive according to claim 1, characterized in that: The catalyst is one or more of stannous octoate, dibutyltin dilaurate, bismuth isooctanoate and zinc isooctanoate.
5. The two-component polyurethane adhesive according to claim 1, characterized in that: The plasticizers in the resin component and the curing agent component are one or more of DBP, DOP, DINP, DOA, DOTP, and TXIP.
6. The two-component polyurethane adhesive according to claim 1, characterized in that: The dewatering agent is p-toluenesulfonyl isocyanate.
7. A method for preparing a two-component polyurethane adhesive, characterized in that: The method is used to prepare the two-component polyurethane adhesive according to any one of claims 1 to 6; the method comprises the following steps: Preparation of resin component: pre-dehydrate all raw materials at high temperature, add other raw materials except catalyst into planetary stirring kettle, stir evenly at room temperature, maintain vacuum for 30-60 minutes, add catalyst after breaking vacuum, continue stirring and dispersing under vacuum for 10-20 minutes, and obtain the resin component; Preparation of curing agent component: Prepolymer, plasticizer and powder are dispersed evenly in a planetary stirring kettle and vacuum is maintained for 30-60 minutes. After breaking the vacuum, dehydrating agent is added and stirring and dispersing is continued for 10-20 minutes under vacuum to obtain the resin component.
8. The preparation method according to claim 7, characterized in that: The preparation method of the prepolymer is as follows: vacuumizing and removing water from the polyol at 120° C. for 1.5-2 hours, cooling to 80-90° C. and breaking the vacuum, then adding one or more of PAPI, MDI, TDI, HMDI, HDI trimer, and IPDI, keeping the temperature for reaction for 2-4 hours, and after the NCO mass content of the reactant reaches 1-9% after testing, cooling and removing bubbles to obtain the NCO-terminated prepolymer.