Method for preparing sulfur-rich polymer by multi-component polymerization of olefins, sulfur and amines

By carrying out multi-component polymerization of sulfur, amine and olefinic monomers at 0-80°C, the problems of insufficient utilization of elemental sulfur and potential safety hazards of high-temperature reactions in the existing technology are solved, and high-yield, low-cost rich-materials are achieved. Preparation of sulfur polymers, polymers with room temperature self-healing and tunable properties.

CN115819767BActive Publication Date: 2024-10-01CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211651554.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-01
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively utilize elemental sulfur to prepare high-sulfur content polymers, and high-temperature reactions lead to safety hazards and low-temperature reaction inertia. There is a lack of multi-component polymerization of olefins, sulfur and amines to prepare sulfur-rich polymers containing "sulfur-sulfur" bonds in the main chain. Polymer methods.

Method used

A multi-component polymerization reaction of sulfur, amine and vinyl monomers is carried out at 0-80°C, and a sulfur-rich polymer is obtained through precipitation and drying. The sulfur element in the polymer exists in the main chain as a "sulfur-sulfur" bond. Adopt a simple and easy method without catalyst, use DMSO, THF or DMF as solvent, and adjust the proportion of monomers to achieve changes in polymer properties.

Benefits of technology

It achieves the preparation of high-yield, low-cost sulfur-rich polymers, reduces the reaction temperature and time, and expands the application of low-boiling point cross-linking agents. The polymer has room temperature self-healing ability and adjustable rigidity and flexibility properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004011366380000021
    Figure BDA0004011366380000021
  • Figure BDA0004011366380000081
    Figure BDA0004011366380000081
  • Figure HDA0004011366390000011
    Figure HDA0004011366390000011
Patent Text Reader

Abstract

The present invention relates to the preparation of sulfur-rich polymers, and specifically discloses a method for preparing sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines, wherein sulfur, amines and olefin monomers are reacted at 0-80°C in bulk or solution. After the reaction is completed, the sulfur-rich polymer is obtained by precipitation and drying. The sulfur element in the sulfur-rich polymer exists in the polymer main chain in the form of a "sulfur-sulfur" bond. The present invention does not require a catalyst and has the characteristics of an autocatalytic reaction. The structural composition and properties of the polymer can be regulated by adjusting the monomer ratio; the reaction monomers are cheap and readily available, the conditions are simple and mild, and the method is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of sulfur-rich polymers, and specifically discloses a method for preparing the sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines. Background Art

[0002] Sulfur is one of the most abundant elements on earth. As a byproduct of hydrodesulfurization in the petroleum refining process in the petrochemical industry, the annual output is as high as tens of millions of tons. Only a small part of this elemental sulfur is used to prepare sulfuric acid or vulcanize rubber, and the vast majority is idle, resulting in huge waste. Moreover, due to its flammable properties, idle sulfur is very likely to cause fires, posing a huge safety hazard. Sulfur has many excellent properties, such as UV absorption, high molar refractive index, high electrode theoretical capacity, sensitive metal detection performance, etc. Therefore, the development of new functional sulfur-rich polymers has become one of the research hotspots.

[0003] At present, the polymerization methods for synthesizing functional materials directly using elemental sulfur as a sulfur source are still very limited. In addition to overcoming the poor physical properties of elemental sulfur and the reaction inertness of elemental sulfur at low temperatures, the low stability of the synthesized high-sulfur-content polymers also needs to be solved urgently. In 2013, Pyun et al. first reported the free radical copolymerization of molten sulfur and 1,3-diisopropylbenzene (DIB) into high-sulfur-content polymers. This polymerization method is called reverse vulcanization reaction. This type of reaction belongs to the free radical polymerization mechanism and needs to be carried out at high temperatures. Later, Tang Benzhong, Hu Rongrong et al. reported a multi-component copolymerization system of sulfur, amines and alkynes or isocyanides. In this reaction, sulfur elements exist in the polymer backbone in the form of thiourea. Lowering the polymerization reaction temperature, expanding the polymerizable monomers, and expanding new synthetic routes for polysulfides have become the focus and difficulty of the sulfur-rich material preparation industry. At present, there is no method for preparing sulfur-rich polymers with a main chain containing "sulfur-sulfur" bonds by multi-component polymerization of olefins, sulfur and amines. Summary of the invention

[0004] In order to solve the shortcomings and deficiencies of sulfur-rich polymer preparation technology, the present invention provides a method for preparing sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines, in which the sulfur element in the prepared sulfur-rich polymer exists in the polymer main chain in the form of "sulfur-sulfur" bonds.

[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0006] The method for preparing sulfur-rich polymer by multi-component polymerization of olefins, sulfur and amines is as follows: sulfur, amine and olefin monomers are reacted at 0-80°C in bulk or solution state. After the reaction is completed, the sulfur-rich polymer is obtained by precipitation and drying. The structural formula of the polymer is as follows:

[0007]

[0008] The olefinic monomer is a monoolefin, a diene, or other multifunctional vinyl monomers.

[0009] Monoolefins are methyl acrylate (MA), n-butyl acrylate (BA), phenyl acrylate (PA), benzyl acrylate (BNA), acrylamide (AM), and N,N-dimethylacrylamide (DMAA);

[0010] The diene is 1,2-hexanediol diacrylate (EGDA), 1,4-butanediol diacrylate (BDDA), polyethylene glycol diacrylate (PEGDA), polycaprolactone diacrylate (PCLDA);

[0011] Other multifunctional vinyl monomers include trimethylolpropane triacrylate (TPTA) and multifunctional polyethylene glycol acrylate (PEG-xMA).

[0012] The amino monomer is a monoamine, a diamine, or other multifunctional amines.

[0013] Among them, the monoamines are n-butylamine (BA), benzylamine (BzA), ethylamine (EA), heptylamine (HA), and aniline (AL);

[0014] The diamines are 1,6-hexanediamine (HDA), 1,12-dodecanediamine (DAD), 1,4-cyclohexanediamine (CHDA), 4,4'-diaminodicyclohexylmethane (DHDA), p-phenylenediamine (PDA), 4,4'-diaminodiphenylmethane (MLDA), and 1,3-phenylenediamine (MXDA);

[0015] Other polyfunctional amines include polyethyleneimine (PEI), Priamine 1071.

[0016] The monomer feed mass ratio is 10-60wt% of olefin monomer, 5-40wt% of elemental sulfur and 5-50wt% of ammonia.

[0017] The solvent used for solution polymerization is dimethyl sulfoxide (DMSO), tetrahydrofuran (THF) or dimethylformamide (DMF).

[0018] The advantages of the present invention compared to the prior art are as follows:

[0019] 1. The elemental sulfur S in the present invention is industrial waste or natural product, which is cheap and abundant, environmentally friendly and harmless, and low in price;

[0020] 2. The present invention does not require a catalyst, has simple and mild conditions, and is simple and easy to implement. It avoids the release of toxic gas hydrogen sulfide caused by the high-temperature reaction process, and greatly expands the application of a large number of low-boiling point cross-linking agents (such as methyl acrylate) such as monoolefins that cannot be used due to high reaction temperatures;

[0021] 3. The method for preparing sulfur-rich polymers by multi-component copolymerization provided by the present invention is a one-step synthesis with high yield and high atomic utilization, which greatly reduces the time and economic cost of polysulfide polymer synthesis;

[0022] 4. The method for preparing sulfur-rich polymers by multi-component copolymerization provided by the present invention, the structure and properties of the polymers can be regulated by adjusting the monomer ratio to achieve the change from rigid materials (50MPa, 10%) to flexible materials (20MPa, 700%);

[0023] 5. The method for preparing sulfur-rich polymers by multi-component copolymerization provided by the present invention, the primary amine, secondary amine or tertiary amine in the polymer structure has a catalytic effect, which can reduce the activation energy of the dynamic exchange of disulfide bonds, enhance the exchange rate of disulfide bonds, and reduce the temperature and time of polymer reprocessing;

[0024] 6. The method for preparing sulfur-rich polymers by multi-component copolymerization provided by the present invention contains a large number of disulfide bonds or polysulfide bonds in the polymer structure, which can be dynamically exchanged at room temperature under the catalysis of primary amines, secondary amines or tertiary amines, so the polymer material has the ability of self-repair at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 FTIR spectra of the product of Example 1 and elemental sulfur.

[0026] Figure 2 DSC curves of the products of Examples 1, 2, 3, and 5

[0027] Figure 3 TG curves of the products of Examples 1, 2, 3, and 5

[0028] Figure 4 1, 2, 12 and 14 are tensile stress-strain curves of the products.

[0029] Figure 5 The XRD spectra of the product of Example 1 and elemental sulfur.

[0030] Figure 6 The XRD spectra of the product of Example 5 and elemental sulfur.

[0031] Figure 7 These are the stress relaxation curves of the products Poly(BDDA-DHDA-S) and P(BDDA-DHDA) of Example 1 at 60°C.

[0032] Figure 8 SEM images of the product of Example 1 before and after self-repair at room temperature: (1) before self-repair, (2) after self-repair at room temperature for 48 hours. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] Weigh 0.13 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 0.85 mL of 4-butanediol diacrylate (BDDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature under inert gas protection for 6 h. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven to give a yield of 96.35 wt%.

[0036] The dried products were subjected to FTIR, DSC, TG, XRD and tensile tests.

[0037] Example 2

[0038] Weigh 0.50 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 0.85 mL of 4-butanediol diacrylate (BDDA) and 5 mL of THF in a 10 mL flask, and stir and react at room temperature under inert gas protection for 6 h. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven to give a yield of 97.54 wt%.

[0039] The dried products were subjected to DSC, TG and tensile tests.

[0040] Example 3

[0041] Weigh 0.63 g of elemental sulfur powder, 4.00 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 10.60 mL of 4-butanediol diacrylate (BDDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 12 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven to give a yield of 98.11 wt%.

[0042] The dried products were subjected to DSC, TG and tensile tests.

[0043] Example 4

[0044] Weigh 0.50 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 3.40 mL of 4-butanediol diacrylate (BDDA) and 5 mL of THF in a 10 mL flask, and stir and react at room temperature for 12 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield is 96.27 wt% after drying in a vacuum oven.

[0045] After drying, the product was subjected to tensile testing.

[0046] Example 5

[0047] 2.00 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 3.40 mL of 4-butanediol diacrylate (BDDA) and 5 mL of THF were weighed into a 10 mL flask. Under the protection of inert gas, the mixture was stirred and reacted at room temperature for 12 h. After the reaction, the mixture was repeatedly precipitated and washed with a precipitant. After drying in a vacuum oven, the yield reached 92.76 wt%.

[0048] The dried products were subjected to DSC, TG, XRD and tensile tests.

[0049] Example 6

[0050] Weigh 0.50 g of elemental sulfur powder, 0.19 g of 1.12-dodecanediamine (DAD), 0.85 mL of 1.4-butanediol diacrylate (BDDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 12 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield is 92.95 wt% after drying in a vacuum oven.

[0051] After drying, the product was subjected to tensile testing.

[0052] Example 7

[0053] Weigh 0.50 g of elemental sulfur powder, 0.2 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 2.00 mL of polyethylene glycol diacrylate (PEGDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 24 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven to give a yield of 95.14 wt%.

[0054] After drying, the product was subjected to tensile testing.

[0055] Example 8

[0056] Weigh 0.50 g of elemental sulfur powder, 0.19 g of 1.12-dodecanediamine (DAD), 2.00 mL of polyethylene glycol diacrylate (PEGDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 24 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield is 92.73 wt% after drying in a vacuum oven.

[0057] After drying, the product was subjected to tensile testing.

[0058] Example 9

[0059] Weigh 0.50 g of elemental sulfur powder, 0.22 g of p-phenylenediamine (PDA), 1.70 mL of 1.4-butanediol diacrylate (BDDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 24 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield is 94.43 wt% after drying in a vacuum oven.

[0060] After drying, the product was subjected to tensile testing.

[0061] Example 10

[0062] Weigh 0.50 g of elemental sulfur powder, 0.5 mL of polyethyleneimine (PEI), 1.70 mL of 1.4-butanediol diacrylate (BDDA) and 5 mL of THF into a 10 mL flask, and stir and react at room temperature for 24 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield reaches 92.34 wt% after drying in a vacuum oven.

[0063] After drying, the product was subjected to tensile testing.

[0064] Embodiment 11

[0065] Weigh 0.13 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 0.85 mL of 4-butanediol diacrylate (BDDA) and 5 mL of DMSO into a 10 mL flask, and stir and react at room temperature for 6 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield is 96.35 wt% after drying in a vacuum oven.

[0066] After drying, the product was subjected to tensile testing.

[0067] Example 12

[0068] Weigh 0.50g of elemental sulfur powder, 1.10g of 4,4'-diaminodiphenylmethane (MLDA), 1.70mL of 1.4-butanediol diacrylate (BDDA) and 5mL of THF in a 10mL flask, and stir and react at room temperature for 24h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven. The yield reaches 94.54wt%

[0069] After drying, the product was subjected to tensile testing.

[0070] Example 13

[0071] Weigh 0.13 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), 0.85 mL of 4-butanediol diacrylate (BDDA) and 5 mL of DMF into a 10 mL flask, and stir and react at room temperature for 6 h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield reaches 98.35 wt% after drying in a vacuum oven.

[0072] After drying, the product was subjected to tensile testing.

[0073] Embodiment 14

[0074] Weigh 0.20g of elemental sulfur powder, 0.14g of 4,4'-diaminodiphenylmethane (MLDA), 2.0g of polycaprolactone diacrylate (PCLDA) and 10mL of DMSO in a 50mL flask, and stir and react at room temperature for 24h under the protection of inert gas. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and the yield reaches 91.54wt% after drying in a vacuum oven.

[0075] After drying, the product was subjected to tensile testing.

[0076] Embodiment 15

[0077] Weigh 0.13 g of elemental sulfur powder, 0.8 mL of 4,4'-diaminodicyclohexylmethane (DHDA), and 0.85 mL of 4-butanediol diacrylate (BDDA) in a 10 mL flask, and stir and react at 80°C for 6 h under inert gas protection. After the reaction, the mixture is repeatedly precipitated and washed with a precipitant, and dried in a vacuum oven to give a yield of 94.35 wt%.

[0078] After drying, the product was subjected to tensile testing.

[0079] Table 1 is a summary table of mechanical strength data of the products of the examples.

[0080] Table 1

[0081]

[0082] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a sulfur-rich polymer by multi-component polymerization of olefins, sulfur and amines, characterized in that: The method comprises: reacting elemental sulfur, amine and olefin monomer at 0-80°C in bulk or solution state, and obtaining a sulfur-rich polymer by precipitation and drying after the reaction is completed; The amine is a monoamine, a diamine or other multifunctional amine; The olefin monomers are: methyl acrylate, n-butyl acrylate, phenyl acrylate, benzyl acrylate, acrylamide, N,N-dimethylacrylamide, 1,2-hexanediol diacrylate, 1,4-butanediol diacrylate, polyethylene glycol diacrylate, polycaprolactone diacrylate, trimethylolpropane triacrylate, and multifunctional polyethylene glycol acrylate.

2. The method for preparing sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines according to claim 1, characterized in that: The monoamines are n-butylamine, benzylamine, ethylamine, heptylamine and aniline; the diamines are 1,6-hexanediamine, 1,12-dodecanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, p-phenylenediamine, 4,4'-diaminodiphenylmethane and 1,3-phenylenediamine; and the other multifunctional amines are polyethyleneimine or Priamine 1071.

3. The method for preparing sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines according to claim 1, characterized in that: In terms of mass percentage, the olefin monomer comprises 10-60 wt%, elemental sulfur comprises 5-40 wt%, and amine comprises 5-50 wt%.

4. The method for preparing sulfur-rich polymers by multi-component polymerization of olefins, sulfur and amines according to claim 1, characterized in that: The solvent used in the solution state is dimethyl sulfoxide, tetrahydrofuran or dimethylformamide.

5. The sulfur-rich polymer prepared according to the method according to any one of claims 1 to 4, characterized in that: The structural formula of the polymer is as follows: 。