A kind of acrylic acid ester structural adhesive and preparation method thereof
By introducing linear multi-block polymer and adjusting the proportion of Tg monomer, the problem of poor bonding strength of acrylate structural adhesives at high temperatures is solved, and the effect of decreasing strength at high temperatures is achieved, ensuring that the substrate is removable and recyclable. Improves the flexibility and impact resistance of the product.
Patent Information
- Application Number
- CN202211481402.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-24
AI Technical Summary
The existing acrylate structural adhesive has poor bonding strength under high temperature conditions, making it difficult to disassemble at high temperatures, affecting the recycling and reuse of substrates.
Introduce linear multiblock polymers to adjust the proportion of high and low glass transition temperature (Tg) monomers to ensure that the product has a high bonding strength at room temperature. The strength drops to detachable at high temperatures. Disassemble by heating up, and add appropriate tackifiers and promoters to increase product sensitivity.
It achieves the effect of reducing strength to detachable at high temperatures, while ensuring safe recycling of the substrate, meeting the needs of high bonding strength at room temperature and moderate strength at high temperatures, and has good flexibility and impact resistance.
Smart Images

Figure BDA0003961794150000011 
Figure BDA0003961794150000021 
Figure BDA0003961794150000022
Abstract
Description
Technical Field
[0001] The invention belongs to the field of adhesives, and in particular relates to an acrylic structural adhesive and a preparation method thereof. Background Art
[0002] In the prior art, isocyanate and special epoxy resin are used to modify acrylate resin multiple times, forming a multi-block structure with alternating arrangement of polyurethane, epoxy and polyol. The vinyl groups at both ends of the molecule participate in free radical copolymerization reaction, achieving the toughening effect on the molecular structure; it is used as a toughening resin to prepare a two-component flexible acrylate structural adhesive with a volume ratio of 10:1 for LCD screen bonding. The adhesive layer has good flexibility and excellent impact resistance. At the same time, the glass transition temperature of the adhesive layer can be limited by controlling the addition ratio, so that it is easy to repair at low temperature; and a high-stability initiator is used to increase the storage stability of the adhesive.
[0003] In the process of preparing adhesives, multiple synthesis reactions are required, the production process is complicated, and the requirements for equipment and operators are high. This application is optimized by using commercially available products, and the production process is physical mixing, which is simple to operate. Summary of the invention
[0004] The purpose of the present invention is to provide an acrylate structural adhesive composition and a preparation method thereof to solve the problem of poor bonding strength of structural adhesives under high temperature conditions in the prior art. The present invention introduces a linear multi-block polymer and adjusts the ratio of high and low TG monomers to ensure the curing speed and medium and low temperature strength of the product, while improving the sensitivity of the product to medium and high temperatures and reducing the bonding strength of the product at the expected temperature. In order to disassemble by heating when bonding errors occur, the expensive substrate can be recycled and reused.
[0005] The purpose of the present invention can be achieved by the following scheme:
[0006] The present invention provides an acrylate structural adhesive, which comprises two components, a main agent and a curing agent, wherein the volume ratio of the main agent to the curing agent is 10:1;
[0007] The main agent includes the following components in parts by weight:
[0008]
[0009]
[0010] The curing agent includes the following components in parts by weight:
[0011]
[0012] As an embodiment of the present invention, the (meth)acrylate monomer includes one or more mixtures of monofunctional acrylate (methyl methacrylate, tetrahydrofuran methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, 2-phenoxyethyl methacrylate, lauric methacrylate), difunctional acrylate (ethylene glycol dimethacrylate, ethoxylated bisphenol A diacrylate), trifunctional acrylate (trimethylolpropane triacrylate), and multifunctional acrylate. The Tg of the (meth)acrylate monomer is 70-76°C. A combination of multiple (meth)acrylate monomers is preferred to meet the Tg requirement. The combination with the linear multi-block copolymer can ensure that the product has a high bonding strength at room temperature, and the strength drops to a detachable strength at a high temperature of about 80°C without damaging the substrate.
[0013] As an embodiment of the present invention, the stabilizer includes one or more of hydroquinone, naphthoquinone, 2,6-di-tert-butyl-p-(dimethylaminomethyl)phenol, and EDTA tetrasodium salt.
[0014] As an embodiment of the present invention, the linear multi-block polymer includes one or more of a diblock copolymer and a triblock copolymer of methacrylate and acrylate, the diblock copolymer includes one or more of styrene-butadiene (BS) and methyl methacrylate-butyl acrylate (MB); the triblock copolymer includes one or more of styrene-butadiene-styrene (SBS), hydrogenated styrene-butadiene-styrene (SEBS), styrene-isoprene-styrene (SIS), and methyl methacrylate-butadiene-styrene (MBS).
[0015] As an embodiment of the present invention, the tackifier is (meth) acrylate phosphate. The (meth) acrylate phosphate includes one or more of monofunctional, difunctional, and trifunctional (meth) acrylate phosphates, including one or more of P1-M, P2-M, PAM200, and CD5090.
[0016] As an embodiment of the present invention, the accelerator includes any one or more of N,N-dimethyl-p-toluidine, N,N-dimethylaniline, N,N-diethyl-p-toluidine, N,N-dimethyl-o-toluidine, and N,N-dihydroxyethyl-toluidine.
[0017] As an embodiment of the present invention, the paraffin wax is fully refined paraffin wax, including one or a mixture of 52# paraffin wax, 58# paraffin wax, 62# paraffin wax, and 68# paraffin wax.
[0018] As an embodiment of the present invention, the other main agent auxiliary agents include one or more of a defoaming agent, fumed silica, a pigment, and a silane coupling agent.
[0019] As an embodiment of the present invention, the peroxide includes any one or more of benzoyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, and dicumyl peroxide.
[0020] As an embodiment of the present invention, the plasticizer includes one or more of trioctyl trimellitate, dipropylene glycol dibenzoate, diethylene glycol dibenzoate, and trioctyl phosphate. The plasticizer used refers to a plasticizer that is not on the REACH list.
[0021] As an embodiment of the present invention, the epoxy resin includes low-halogen or halogen-free epoxy resin. The epoxy resin includes one or more of bisphenol A epoxy resin (DER331, NPEL 128, NPEL127) and bisphenol F epoxy resin (NPEF170, NPEF-180).
[0022] As an embodiment of the present invention, the resin filler includes one or more of SBS, MBS and SEBS.
[0023] As an embodiment of the present invention, the other curing agent additives include one or more of fumed silica, glass microspheres, hollow microspheres, HDPE particles, pigments, silane coupling agents, water, and zinc stearate.
[0024] The present invention also provides a method for preparing the acrylate structural adhesive composition, the preparation method comprising the following steps:
[0025] S1, main agent component: (meth) acrylate monomer, (meth) acrylic acid and stabilizer are mixed and stirred, melted paraffin and linear multi-block copolymer are added, dispersed evenly and swelled into a uniform paste, and then tackifier, accelerator and other auxiliary agents are added while stirring, and stirred evenly to obtain the main agent component; step S1 controls the temperature to be 20-40°C;
[0026] S2, curing agent component: after the plasticizer and epoxy resin are mixed and stirred evenly, the resin filler is added while stirring, and after the mixture is stirred evenly, it is allowed to stand and swell. After the mixture is fully swollen, the mixture is stirred evenly, and while cooling water is passed, peroxide and other additives are added while stirring, and the mixture is stirred until evenly mixed to obtain a curing agent component; the temperature in step S2 is controlled at 20-40°C;
[0027] S3. Evenly mix the main agent component obtained in step S1 and the curing agent component obtained in step S2 (according to a volume ratio of 10:1) to obtain an acrylate structural adhesive.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) By introducing a linear multi-block copolymer and a combination of monomers with different Tg values (the Tg calculated by the Tg calculation formula is about 75°C, ensuring that the product has a high bonding strength at room temperature, and at a high temperature, about 80°C, the strength drops to a detachable strength without damaging the substrate), the acrylic structural adhesive prepared solves the unacceptable shortcomings of conventional acrylic structural adhesives such as high high-temperature bonding strength, high hardness, and poor flexibility for screen bonding, and obtains a reworkable acrylic structural adhesive that meets the requirements of high bonding strength at room temperature, moderate / low high-temperature strength, good flexibility, and impact resistance.
[0030] (2) The present invention introduces linear multi-block polymers and adjusts the ratio of high and low TG monomers to ensure the curing speed and medium and low temperature strength of the product, while improving the sensitivity of the product to medium and high temperatures and reducing the bonding strength of the product at the expected temperature. In this way, when bonding errors occur, the product can be disassembled by heating, while ensuring the recycling of expensive substrates. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, which will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.
[0032] Examples 1-4
[0033] The monomer content in the main agent is fixed, and the glass transition temperature is calculated according to the glass transition temperature formula, and the glass transition temperature is about 75°C. The type and proportion of the elastomer in the main agent are changed to obtain Examples 1-4 and two reference examples. The same curing agent is used.
[0034] The main composition is as follows:
[0035]
[0036]
[0037] The curing agent composition is as follows
[0038]
[0039] The curing agent and Examples 1-4 and reference were packaged into 10:1 two-component rubber tubes, and the tensile shear strength of ink glass and PC at room temperature and at 80°C were tested according to GB / T 7124-2008. The tensile shear strength of ink glass and PC was tested by hot pressing (glue layer temperature 60°C) for 90s and cooling at room temperature for 1min. The results are as follows:
[0040]
[0041] *: Reduce the bonding area to 1 / 4 of the standard.
[0042] It can be seen that the shear strength of different Tg monomer combinations and linear multi-block polymers after hot pressing is 1.0-1.3MPa, reaching the clamping strength required by the electronics market; the tensile strength at room temperature is 6.5-8.0MPa, which can meet the adhesion requirements of the electronics market; at 80°C, the shear strength is 1.5-2.0MPa, which can be manually peeled without damaging the ink glass, and the ink glass is consistent with the ink glass before use after wiping with non-woven fabric. The shear strength of the reference sample at 80°C is 5.7 and 4.8MPa respectively, which is easy to damage the ink glass during rework.
[0043] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. An acrylic structural adhesive, It is characterized in that The acrylic structural adhesive comprises a main agent and a curing agent; The main agent includes the following components in parts by weight: 40-60 parts of (meth)acrylate monomer; (Meth) acrylic acid 1-5 parts; Stabilizer 0~2 parts; 20-40 parts of linear multi-block polymer; Thickener 1~5 parts; Accelerator 0~5 parts; 1~5 parts of paraffin; Other additives 0~10 parts; The curing agent includes the following components in parts by weight: Peroxide 20~40 parts; Plasticizer 10~40 parts; Epoxy resin 10~40 parts; Resin filler 10~20 parts; Other additives 0~10 parts; The (meth)acrylate monomer is a combination of methyl methacrylate, tetrahydrofuran methacrylate and lauric methacrylate; the Tg of the (meth)acrylate monomer is 70-76°C; The linear multi-block polymer is a combination of styrene-butadiene-styrene, methyl methacrylate-butadiene-styrene and hydrogenated styrene-butadiene-styrene.
2. The acrylate structural adhesive according to claim 1, It is characterized in that The stabilizer includes one or more of hydroquinone, naphthoquinone, 2,6-di-tert-butyl-p-(dimethylaminomethyl)phenol, and EDTA tetrasodium salt.
3. The acrylate structural adhesive according to claim 1, It is characterized in that The tackifier is (meth)acrylic acid phosphate.
4. The acrylate structural adhesive according to claim 1, It is characterized in that The accelerator includes any one or more of N,N-dimethyl-p-toluidine, N,N-dimethylaniline, N,N-diethyl-p-toluidine, N,N-dimethyl-o-toluidine, and N,N-dihydroxyethyl-toluidine.
5. The acrylate structural adhesive according to claim 1, It is characterized in that The paraffin wax is fully refined paraffin wax, including one or a mixture of 52# paraffin wax, 58# paraffin wax, 62# paraffin wax, and 68# paraffin wax.
6. The acrylate structural adhesive according to claim 1, It is characterized in that The other auxiliary agents include one or more of a defoamer, fumed silica, a pigment, and a silane coupling agent.
7. The acrylate structural adhesive according to claim 1, It is characterized in that The peroxide includes any one or more of benzoyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, and dicumyl peroxide.
8. A method for preparing the acrylic structural adhesive according to claim 1, It is characterized in that The preparation method comprises the following steps: S1. Main agent component: (meth)acrylate monomer, (meth)acrylic acid and stabilizer are mixed and stirred, melted paraffin and linear multi-block polymer are added, dispersed evenly and swelled into a uniform paste, and then tackifier, accelerator and other additives are added while stirring, and stirred evenly to obtain the main agent component; S2, curing agent component: after the plasticizer and epoxy resin are mixed and stirred evenly, the resin filler is added while stirring, and after the mixture is stirred evenly, it is allowed to stand and swell. After the mixture is fully swollen, the mixture is stirred evenly, and while cooling water is passed, peroxide and other additives are added while stirring, and the mixture is continued to be stirred until evenly mixed, thereby obtaining a curing agent component; S3, the main agent component prepared in step S1 and the curing agent component prepared in step S2 are mixed uniformly to obtain an acrylate structural adhesive.
Citation Information
Patent Citations
Low-water-absorptivity acrylate structural adhesive and preparation method thereof
CN102850973A
High-elasticity room temperature rapidly cured acrylic ester structure adhesive and preparation method thereof
CN103571406A
Ultrahigh-strength acrylate structural adhesive with wide adhesion and preparation method of ultrahigh-strength acrylate structural adhesive
CN104449418A
Acrylate adhesive for bonding resin-based composite material and preparation method of acrylate adhesive
CN111087953A
Bi-component acrylate structural adhesive
CN114752308A