A soft elastic abrasive grain for tool polishing and passivation processing and a preparation method thereof
By using hard abrasives and soft elastic abrasive grains embedded in a soft carrier on the tool surface, the problems of low tool passivation efficiency and poor precision in the existing technology are solved, and efficient and accurate polishing and passivation integrated processing is achieved, improving Improves tool surface quality and abrasive grain service life.
Patent Information
- Application Number
- CN202211391321.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-08
AI Technical Summary
The existing tool passivation technology has low processing efficiency and poor precision. It cannot take into account the integrated processing of polishing and passivation of carbide and superhard material tools, and the quality is uneven and stable.
It uses soft elastic abrasive grains with a "core-shell" structure that are evenly embedded in the surface of the soft carrier by hard abrasives. They are ejected at high speed through the spray gun and collide with the surface to be treated. The elastic deformation of the soft carrier is used to produce scratching, rolling and plowing. Plow effect, achieving both passivation and polishing functions.
It achieves high-efficiency and high-precision integrated processing of tool polishing and passivation. The processed tool has low surface roughness, obvious edge arc, high surface quality, low sub-surface damage, and long service life of soft elastic abrasive grains, which is suitable for large applications. Mass production.
Smart Images

Figure CN115820209B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flexible abrasive grain manufacturing, and specifically relates to a method for preparing soft elastic abrasive grains, in particular to soft elastic abrasive grains used for integrated polishing and passivation processing of cemented carbide and superhard material tools and a method for preparing the same. Background Art
[0002] As a cutting edge post-processing technology, tool passivation technology is one of the essential processes in modern tool manufacturing. This processing technology is a process that uses appropriate process methods to eliminate various defects in the cutting edge and the cutting edge micro-area, and obtain appropriate cutting edge micro-geometric parameters and surface morphology. After tool passivation treatment, the residual stress of the cutting edge can be eliminated, the cutting edge strength can be improved, the coating adhesion can be increased, the wear resistance of the cutting edge can be improved, and finally the stability and life of the tool can be improved.
[0003] At present, the mature types of tool passivation technologies and process methods at home and abroad mainly include abrasive brush method, vertical rotation method, micro-abrasive sandblasting method and magnetic powder passivation method. Among them, the abrasive brush method will produce uneven edge radius defects when passivating rotary tools, and the passivation quality is not stable enough; the vertical rotation method will have uneven edge radius along the axial direction, and the polishing effect on superhard tools is limited, and the tool surface polishing is uneven; the micro-abrasive sandblasting method will etch the surface of superhard material tools and reduce the surface smoothness; the magnetic powder passivation method cannot process contour tools, and the outer diameter of the tool changes greatly, and the price is high.
[0004] In summary, the existing tool surface treatment technology has the problems of low processing efficiency and poor processing accuracy; it is unable to take into account both carbide and superhard material tools; it is difficult to integrate passivation and polishing into one process with uniform and stable quality. Therefore, the core content of this invention is to research and invent a soft elastic abrasive for high-quality and efficient polishing and passivation of tools. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a soft elastic abrasive with a "core-shell" structure uniformly embedded in the surface of a soft carrier, which is used for tool polishing and passivation processing. When the abrasive is used for tool surface treatment, the abrasive collides with the tool surface and its soft carrier is deformed, which causes the abrasive to produce a certain scratching, rolling and plowing effect on the tool surface, and removes the surface material in a fine manner, finally realizing high-efficiency and high-precision polishing and passivation integrated processing.
[0006] The second object of the present invention is to provide a method for preparing the soft elastic abrasive grains used in tool polishing and passivation processing.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A method for preparing soft elastic abrasive grains for tool polishing and passivation processing comprises the following steps:
[0009] S1. Processing of polymer viscoelastic substrate: crushing and sieving the polymer viscoelastic substrate masterbatch to obtain soft carrier particles within the target particle size range and target shape;
[0010] S2. Preparation of multi-component abrasives: Mix and sieve a certain proportion of superhard abrasives and ordinary abrasives to obtain evenly dispersed multi-component abrasives;
[0011] S3, heating the soft carrier particles: pouring the soft carrier particles prepared in S1 into a heatable mixing device, and stirring them at a certain temperature for a certain period of time, through the continuous rotation stirring and heating of the device, ensuring that the soft carrier particles do not agglomerate and produce a certain degree of viscosity-flow transition on their surface;
[0012] S4, preparation of soft carrier / hard abrasive composite particles: pouring the multi-component abrasives of S2 evenly into the soft carrier particle system obtained in S3 according to a certain proportion, stirring continuously for a certain period of time by a heatable mixing device, so that the hard abrasives are compacted and evenly distributed on the surface of the soft carrier, and preparing soft carrier / hard abrasive composite particles;
[0013] S5. Post-processing of soft carrier / hard abrasive composite particles: The composite particles prepared in S4 are collected and placed at room temperature for a certain period of time, and then sieved repeatedly to obtain soft elastic abrasive particles within the target particle size range and in the target shape.
[0014] Specifically, in step S1, the Shore hardness of the polymer viscoelastic substrate masterbatch is less than or equal to 70HA, and the density range is 0.6-2.2g / cm 3 The polymer viscoelastic substrate masterbatch can be specifically selected from one or more of natural rubber (NR), isoprene rubber (IR), polyurethane rubber (PUR), styrene thermoplastic elastomer (TPES), thermoplastic polyurethane (TPU), ethylene-vinyl acetate copolymer and polyolefin elastomer (POE).
[0015] Furthermore, in step S1, the target particle size range of the soft carrier particles is 0.2-0.8 mm, and the target shape is flat and / or cubic.
[0016] Specifically, in step S2, in terms of mass percentage, the superhard abrasive is 40-60%, and the common abrasive is 40-60%, that is, the sum of the mass percentages of the superhard abrasive and the common abrasive is 100%. The superhard abrasive is selected from one or more of diamond, cubic boron nitride, etc.; the common abrasive is selected from one or more of zirconium oxide, silicon oxide, cerium oxide, silicon carbide, boron carbide, white corundum, brown corundum, etc.
[0017] Furthermore, the particle size of the multi-component abrasive is 0.1-4.0 μm.
[0018] Specifically, in step S3, the setting temperature of the heated mixing device is 20-40°C below the viscosity-flow transition temperature of the soft carrier particles, that is, the setting temperature is 20-40°C lower than the viscosity-flow transition temperature of the soft carrier particles; the stirring time is 10-15min.
[0019] Furthermore, in step S4, when preparing the soft carrier / hard abrasive composite particles, by mass percentage, the multi-component abrasive is 10-25%, and the soft carrier particles are 75-90%, that is, the sum of the mass percentages of the multi-component abrasive and the soft carrier particles is 100%; the stirring time is 25-45 min.
[0020] Specifically, in step S5, the room temperature is in the range of 25±5° C., and the standing time is 4-6 hours. The target particle size of the obtained soft elastic abrasive particles is in the range of 0.2-0.8 mm, and the target shape is flat and / or cubic.
[0021] The present invention also provides soft elastic abrasive grains for tool polishing and passivation processing prepared by the above preparation method. The soft elastic abrasive grains for tool polishing and passivation processing include:
[0022] The soft carrier is made of a macromolecular viscoelastic material and has excellent elasticity. As the main body of the soft elastic abrasive, it can undergo elastic deformation when subjected to external forces and is used to fix, embed, and support hard abrasives.
[0023] The hard abrasive is composed of ordinary abrasive and super-hard abrasive. Through the rotating stirring action of the mixing device, its sharp edges penetrate into the soft carrier and are embedded in the surface of the soft carrier to be used for grinding the surface material of the workpiece to be processed.
[0024] The soft elastic abrasive of the present invention has excellent elasticity based on the unique viscoelasticity of the polymer material-based soft carrier. The soft elastic abrasive of the present invention is sprayed out at high speed through a spray gun and collides with the surface to be processed. The abrasive stores a certain elastic potential energy, which is released after the abrasive and the workpiece surface have a certain sliding motion, so that the soft elastic abrasive can restore its original shape and bounce off the surface to be processed at the same time, finally achieving the two functions of passivation and polishing. The hard abrasive is tightly embedded in the surface of the soft carrier and can effectively participate in the processing of the workpiece. The soft elastic abrasive tool prepared by the present invention has low surface roughness, obvious cutting edge arc, no chipping, high surface quality and low sub-surface damage after processing.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1) The soft elastic abrasive grains of the present invention have a relatively large specific gravity and excellent elasticity. They are matched with conventional negative pressure suction blasting equipment in the field, are sucked into the spray gun and mixed with the airflow, and are sprayed out from the nozzle through compressed air. They can scratch, roll and plow on the surface of the workpiece at a certain speed and pressure, and remove the surface material in a fine manner, thereby reducing the roughness of the workpiece surface;
[0027] 2) The soft elastic abrasive particles of the present invention are sharp, have obvious edges and corners, and are flat and cubic particles. When the overall ejection speed of the soft elastic abrasive particles is the same, the soft elastic abrasive particles can collide with the surface of the workpiece with a smaller contact area, resulting in a single abrasive particle generating a greater pressure, a larger amount of material removal, and a deeper scratch, that is, a more obvious polishing passivation effect;
[0028] 3) The soft elastic abrasive of the present invention can significantly enhance the interlocking effect between the soft carrier and the hard abrasive by the soft carrier itself undergoing a micro-viscous flow state-high elastic state-glass state transition to embed the hard abrasive, thereby increasing the overall service life of the soft elastic abrasive, specifically, the soft elastic abrasive can work continuously for 800 hours or more;
[0029] 4) The soft elastic abrasive of the present invention has simple processing operation, high processing efficiency and good processing effect. It can process complex 3D curved surfaces such as tool surfaces, grooves, depressions and slits, and can passivate all positions of the tool edge evenly. The roughness of the workpiece after processing is Ra≤0.05μm, the arc size of the cutting edge after processing is 5-12μm, and there are no scratches on the tool surface, which fully meets the technical index requirements of tool polishing and passivation.
[0030] 5) The soft elastic abrasive grains of the present invention have low cost of raw materials and manufacturing equipment, simple and stable preparation process, and are easy to mass produce and promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 It is a specific process flow diagram of the present invention;
[0033] Figure 2 This is a SEM schematic diagram of the soft elastic abrasive particles of the present invention;
[0034] Figure 3 Schematic diagram of the processing principle of the soft elastic abrasive particles of the present invention;
[0035] In the figure: 1. Spray gun; 2. Processing workpiece surface; 3. Surface grinding layer; 4. Soft carrier; 5. Hard abrasive;
[0036] Figure 4 The schematic diagram of the soft elastic abrasive grains of the present invention for machining a φ8 solid carbide drill before and after processing; in the figure: 1, unprocessed workpiece; 2, processed workpiece;
[0037] Figure 5 This is a SEM schematic diagram of the soft elastic abrasive in comparative example 1. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Unless otherwise specified, the raw materials used in the examples are all common commercial products that can be directly purchased in the art. Room temperature refers to 25±5°C.
[0040] Example 1
[0041] Thermoplastic polyurethane-based soft elastic abrasive with a particle size range of 0.4-0.8 mm was prepared. The raw materials were made of thermoplastic polyurethane (TPU), boron carbide and diamond. The mass percentage and type of each raw material are shown in Table 1.
[0042] Table 1 Mass percentage and type of each raw material
[0043]
[0044] The preparation method of the above soft elastic abrasive grains (process flow chart see Figure 1 ), specifically including the following steps:
[0045] S1. Processing of thermoplastic polyurethane substrate: Crushing thermoplastic polyurethane masterbatch based on freeze crushing granulation process. The freeze crushing granulation process is a conventional material processing method in this field. The specific process is: first, soak the thermoplastic polyurethane masterbatch in a liquid nitrogen environment at -140°C for 5 minutes, and then use the feeding rod to send the thermoplastic polyurethane masterbatch in a glassy state to the crushing chamber of the hammer crushing equipment, and collect the product through processing. Subsequently, pass the product through a 20# sieve and use a 40# sieve to receive it, and collect the thermoplastic polyurethane particles in the 40#-20# range, that is, collect the soft carrier thermoplastic polyurethane particles with a particle size range of 0.4-0.8mm and flat and cubic shapes;
[0046] S2. Preparation of multi-component abrasive: 45 g of boron carbide with a specification of W0.5 and 45 g of diamond powder with a specification of M0 / 2 are put into a glass container, stirred and mixed repeatedly, and sieved through a 80# sieve for 3 times to obtain a multi-component abrasive with a uniformly dispersed particle size range of 0.1-2.5 μm;
[0047] S3, heating of thermoplastic polyurethane particles: add 500g of thermoplastic polyurethane particles collected in S1 into a mixing barrel with a diameter of 500mm and a height of 800mm, and place the mixing barrel in a heated rotary mixer (this is a conventional device in the art, mainly with heating and rotary mixing functions, which can be purchased directly. Since its structure is not the innovation of this application, it will not be described in detail). Set the temperature to 130°C and stir for 10 minutes to obtain thermoplastic polyurethane particles with a certain degree of viscosity-flow transition on the surface;
[0048] S4, preparation of thermoplastic polyurethane-based soft elastic abrasive particles: 80g of the multi-component abrasive obtained in S2 is poured into the thermoplastic polyurethane particle system with a micro-viscous flow transition on the surface obtained in S3. The mixture is continuously shaken and stirred for 30 minutes by a heated rotary mixer to compact and evenly distribute the hard abrasive on the surface of the thermoplastic polyurethane, thus preparing thermoplastic polyurethane-based composite particles with hard abrasives evenly embedded on the surface;
[0049] S5, post-treatment of thermoplastic polyurethane-based soft elastic abrasive particles: collect the product prepared in S4 and place it at room temperature for 5 hours. Then, pass the product through a 20# sieve and use a 40# sieve to collect the thermoplastic polyurethane-based soft elastic abrasive particles in the 40#-20# range, and obtain thermoplastic polyurethane-based soft elastic abrasive particles with a particle size range of 0.4-0.8 mm.
[0050] Figure 2 The SEM schematic diagram of the soft elastic abrasive prepared in this example is given. It can be seen from the figure that the thermoplastic polyurethane-based soft elastic abrasive is sharp, has obvious edges and corners, and is in the form of cubic particles; and the soft elastic abrasive has a uniform particle size distribution, wherein the particle size shown in the figure is about 0.6 mm.
[0051] Figure 3A schematic diagram of the processing principle of the soft elastic abrasive of the present invention is given; in the figure: 1, spray gun; 2, surface of the workpiece to be processed; 3, surface grinding layer; 4, soft carrier; 5, hard abrasive. Specifically, the soft elastic abrasive of the present invention is sucked into the spray gun 1 and mixed with the airflow, and is ejected from the nozzle in the form of a jet through compressed air, with an initial speed of more than 80m / s, so that the soft elastic abrasive is accelerated and obtains kinetic energy. Subsequently, the soft elastic abrasive reaches the surface 2 of the workpiece to be processed, collides with the workpiece to cause deceleration, and the soft elastic abrasive produces a large compression based on its excellent elasticity and stretches and rolls along the surface of the workpiece, and the kinetic energy of the soft elastic abrasive is converted into elastic potential energy and stored. When the elastic potential energy is released, the soft elastic abrasive restores its original shape and bounces off the surface of the workpiece at the same time, and then detaches from the surface of the workpiece. The collision of the soft elastic abrasive with the workpiece and the "compression-elongation-bounce" on the surface of the workpiece produce a scratching and plowing effect on the surface of the workpiece, thereby removing the material on the surface of the workpiece to achieve the purpose of integrated passivation and polishing processing.
[0052] The soft elastic abrasive prepared in this example was used with conventional negative pressure suction blasting equipment in the field to perform a surface polishing experiment on a φ8 solid carbide drill. The process parameters were as follows: the blasting air pressure was set to 0.35 MPa; the workpiece was processed in a forward and reverse, up and down movement mode, the speed was set to 30.0 RPM; the spray gun spray angle was 45°.
[0053] Figure 4 The front and back schematic diagrams of the soft elastic abrasive prepared in this example machining a φ8 solid carbide drill are given. Using the above process parameters, when the number of forward and reverse rotations reaches 20 times, the total machining time is 5.5 minutes, and the machining of the tool can be completed. The surface of the tool after machining is tested, and the surface roughness value Ra≤0.05μm; the arc size range of the cutting edge reaches 0.005-0.012mm; there are no scratches on the tool surface (see Figure 4 ), fully meeting the technical requirements of tool polishing and passivation.
[0054] Example 2
[0055] Natural rubber-based soft elastic abrasive with a particle size range of 0.2-0.4 mm was prepared. The raw materials consisted of natural rubber (NR), zirconium oxide, cerium oxide and diamond. The mass percentage and type of each raw material are shown in Table 2.
[0056] Table 2 Mass percentage and type of each raw material
[0057]
[0058] The method for preparing the soft elastic abrasive grains specifically comprises the following steps:
[0059] S1. Processing of natural rubber substrate: crushing natural rubber masterbatch based on the freezing crushing granulation process. The freezing crushing granulation process is a conventional material processing method in this field. The specific process is: first, soak the natural rubber masterbatch in a liquid nitrogen environment at -140°C for 5 minutes, and then use the feeding rod to send the natural rubber masterbatch in a glassy state to the crushing chamber of the hammer crushing equipment, and collect the product through processing. Subsequently, pass the product through a 40# sieve and use a 60# sieve to receive the natural rubber particles in the 60#-40# range, that is, collect the soft carrier natural rubber particles with a particle size range of 0.2-0.4mm and flat and cubic shapes;
[0060] S2. Preparation of multi-component abrasive: 40 g of zirconium oxide with a specification of W3.5, 40 g of cerium oxide with a specification of W3.5 and 55 g of diamond powder with a specification of M1 / 2 were put into a glass container, stirred and mixed repeatedly, and sieved through a 80# sieve for 3 times to obtain a multi-component abrasive with a uniformly dispersed particle size range of 1.0-3.5 μm;
[0061] S3, heating of natural rubber particles: add 800g of the natural rubber particles collected in S1 into a mixing barrel with a diameter of 500mm and a height of 800mm, and place the mixing barrel in a heated rotary mixer. Set the temperature to 80℃ and stir for 10min to obtain natural rubber particles with a certain degree of viscosity flow transition on the surface;
[0062] S4, preparation of natural rubber-based soft elastic abrasive particles: 120 g of the multi-component abrasive obtained in S2 is poured into the natural rubber particle system with a micro-viscous flow transition on the surface obtained in S3. The mixture is continuously shaken and stirred for 40 minutes by a heated rotary mixer to compact and evenly distribute the hard abrasive on the surface of the natural rubber, thus preparing natural rubber-based composite particles with hard abrasives evenly embedded on the surface;
[0063] S5, post-treatment of natural rubber-based soft elastic abrasive particles: collect the product prepared in S4 and place it at room temperature for 4 hours. Then, pass the product through a 40# sieve and use a 60# sieve to collect the natural rubber-based soft elastic abrasive particles in the 60#-40# range, and obtain natural rubber-based soft elastic abrasive particles with a particle size range of 0.2-0.4 mm.
[0064] The processing effect of the soft elastic abrasive prepared in Example 2 is the same as that in Example 1.
[0065] Example 3
[0066] The styrene-based thermoplastic elastomer-based soft elastic abrasive with a particle size range of 0.4-0.8 mm is prepared. The raw materials are composed of styrene-based thermoplastic elastomer, specifically styrene-butadiene-styrene block copolymer (SBS), green silicon carbide and cubic boron nitride. The mass percentage and type of each raw material are shown in Table 3.
[0067] Table 3 Mass percentage and type of each raw material
[0068]
[0069] The method for preparing the soft elastic abrasive grains specifically comprises the following steps:
[0070] S1. Processing of styrene-butadiene-styrene block copolymer substrate: crushing styrene-butadiene-styrene block copolymer masterbatch based on the freeze crushing granulation process. The freeze crushing granulation process is a conventional material processing method in this field. The specific process is: first, immerse the styrene-butadiene-styrene block copolymer masterbatch in a -140°C liquid nitrogen environment for 5 minutes, and then use the feeding rod to send the glassy styrene-butadiene-styrene block copolymer masterbatch to the crushing chamber of the hammer crushing equipment, and collect the product through processing. Subsequently, pass the product through a 20# sieve and use a 40# sieve to receive the styrene-butadiene-styrene block copolymer particles in the 40#-20# range, that is, collect the soft carrier styrene-butadiene-styrene block particles with a particle size range of 0.4-0.8mm and flat and cubic shapes;
[0071] S2. Preparation of multi-component abrasive: 175 g of green silicon carbide micropowder with a specification of W2.5 and 255 g of cubic boron nitride micropowder with a specification of M1 / 3 were put into a glass container, stirred and mixed repeatedly, and sieved through a 80# sieve for 3 times to obtain a multi-component abrasive with a uniformly dispersed particle size range of 2.0-4.0 μm;
[0072] S3, heating of styrene-butadiene-styrene block copolymer particles: add 2000g of styrene-butadiene-styrene block copolymer particles collected in S1 into a mixing barrel with a diameter of 800mm and a height of 1500mm, and place the mixing barrel in a heated rotary mixer. Set the temperature to 120°C and stir for 15 minutes to obtain styrene-butadiene-styrene block copolymer particles with a certain degree of viscosity-flow transition on the surface;
[0073] S4, preparation of styrene-butadiene-styrene block copolymer-based soft elastic abrasive particles: 420 g of the multi-component abrasive obtained in S2 is poured into the styrene-butadiene-styrene block copolymer particle system with a micro-viscous flow transition on the surface obtained in S3. The hard abrasive is compacted and evenly distributed on the surface of the styrene-butadiene-styrene block copolymer by continuous shaking and stirring in a heated rotary mixer for 40 minutes, so as to obtain styrene-butadiene-styrene block copolymer-based composite particles with hard abrasives evenly embedded on the surface;
[0074] S5. Post-treatment of styrene-butadiene-styrene block copolymer-based soft elastic abrasive grains: The product prepared in S4 was collected and placed at room temperature for 6 hours. Subsequently, the product was passed through a 20# sieve and received with a 40# sieve, and styrene-butadiene-styrene block copolymer-based soft elastic abrasive grains in the 40#-20# range were collected to obtain styrene-butadiene-styrene block copolymer-based soft elastic abrasive grains with a particle size range of 0.4-0.8 mm.
[0075] The processing effect of the soft elastic abrasive prepared in Example 3 is the same as that in Example 1.
[0076] Comparative Example 1
[0077] The difference between this comparative example 1 and example 1 is that the flat and cubic soft carrier thermoplastic polyurethane particles in example 1 are replaced with rounded and non-angular soft carrier thermoplastic polyurethane particles. The preparation process is the same as that in example 1.
[0078] The SEM image of the elastic abrasive prepared in this comparative example 1 is shown in Figure 5 .Depend on Figure 5 It can be seen from the figure that the thermoplastic polyurethane-based elastic abrasive particles are round in shape and have no obvious edges or corners.
[0079] Subsequently, the thermoplastic polyurethane-based elastic abrasive prepared in Comparative Example 1 was used in conjunction with a negative pressure suction-jet sandblasting device, and the same processing parameters as in Example 1 were used to perform polishing and passivation processing on a φ8 solid carbide drill. The processing results are shown in Table 4 below.
[0080] Table 4 Polishing and passivation processing effects of the products of Example 1 and Comparative Example 1 on φ8 solid carbide drill
[0081]
[0082] It can be seen from Table 4 that the soft elastic abrasive particles (Example 1) prepared by using the flat and cubic soft carrier thermoplastic polyurethane particles of the present invention, under the same processing technology, have significantly better surface roughness and cutting edge arc size of the processed workpiece than the soft elastic abrasive particles (Comparative Example 1) prepared by using the rounded and non-angular soft carrier thermoplastic polyurethane particles. That is to say, the soft elastic abrasive particles of the present invention are sharp, have obvious edges and corners, are flat and cubic particles, so that when the overall ejection speed of the soft elastic abrasive particles is the same, the soft elastic abrasive particles can collide with the workpiece surface with a smaller contact area, resulting in a single abrasive particle generating greater pressure, a larger amount of material removal, and deeper scratches, that is, the polishing passivation effect is more obvious.
[0083] Comparative Example 2
[0084] The difference between this comparative example and Example 1 is that a different preparation process is adopted from that of Example 1.
[0085] The preparation method of the elastic abrasive in this comparative example is: by spraying an adhesive atomized on the surface of rolling soft carrier particles, then mixing the multi-component abrasive with the soft carrier particles adhered with the adhesive, and compacting the multi-component abrasive on the surface of the soft carrier particles by centrifugal force or impact force to prepare elastic abrasive (Comparative Example 2).
[0086] Subsequently, the elastic abrasive prepared in Comparative Example 2 was used in conjunction with a negative pressure suction blasting equipment, and the same processing parameters as in Example 1 were used to perform polishing and passivation processing on the φ8 solid carbide drill. The processing results are shown in Table 5 below.
[0087] Table 5 The processing effect of polishing and passivation of φ8 solid carbide drill by using Example 1 and Comparative Example 2
[0088]
[0089] It can be seen from Table 5 that the elastic abrasive (Comparative Example 2) obtained by connecting the soft carrier and the hard abrasive using an adhesive as an intermediate medium has a processing effect equivalent to that of Example 1 at the initial stage of processing. However, with the increase of continuous working time, the processing effect of Comparative Example 2 gradually deteriorates, and after 300-500 hours of processing, the soft elastic abrasive loses its processing ability. That is to say, compared with the soft elastic abrasive (Comparative Example 2) obtained by using an atomized adhesive, the soft elastic abrasive obtained by the present invention based on the self-adhesion of the polymer viscoelastic substrate has a stronger interlocking effect between the soft carrier and the hard abrasive, and thus the soft elastic abrasive of the present invention has a better continuous processing effect and a longer service life.
[0090] In summary, it can be seen that the soft elastic abrasive particles of the present invention, which are made of hard abrasives and are uniformly embedded on the surface of a soft carrier, are used for polishing and passivation of tool surfaces. When the abrasive particles collide with the tool surface, the soft carrier thereof will be deformed, thereby causing the abrasive particles to produce certain scratching, rolling and plowing effects on the tool surface, and to remove the surface material in a fine manner, and finally realize high-efficiency and high-precision integrated polishing and passivation processing. The soft elastic abrasive particles prepared by the present invention can effectively solve the technical problems existing in the existing tool surface treatment technology, such as low processing efficiency, poor precision, difficulty in integrating polishing and passivation processing, and uniform and stable quality, greatly improve the processing efficiency, and have a high promotion value.
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing soft elastic abrasive grains for tool polishing and passivation processing, characterized in that: The steps include: S1. Thermoplastic polyurethane substrate processing: The thermoplastic polyurethane masterbatch is crushed based on the freezing crushing granulation process. The specific process is: first, the thermoplastic polyurethane masterbatch is immersed in a liquid nitrogen environment at -140°C for 5 minutes, and then the thermoplastic polyurethane masterbatch in a glassy state is sent to the crushing chamber of a hammer crushing equipment through a feeding rod, and the product is collected through processing; Then, the product is passed through a 20# sieve and a 40# sieve is used to receive the thermoplastic polyurethane particles in the 40#-20# range, that is, the soft carrier thermoplastic polyurethane particles with a particle size range of 0.4-0.8 mm and a flat or cubic shape are collected; S2. Preparation of multi-component abrasive: 45 g of boron carbide with a specification of W0.5 and 45 g of diamond powder with a specification of M0 / 2 are put into a glass container, stirred and mixed repeatedly, and sieved through a 80# sieve for 3 times to obtain a multi-component abrasive with a uniformly dispersed particle size range of 0.1-2.5 μm; S3, heating the thermoplastic polyurethane particles: add 500 g of the thermoplastic polyurethane particles collected in S1 into a mixing barrel with a diameter of 500 mm and a height of 800 mm, and place the mixing barrel in a heated rotary mixer; set the temperature to 130° C. and stir for 10 minutes to obtain thermoplastic polyurethane particles with a certain degree of viscosity-flow transition on the surface; S4, preparation of thermoplastic polyurethane-based soft elastic abrasive particles: 80 g of the multi-component abrasive obtained in S2 is poured into the thermoplastic polyurethane particle system with a micro-viscous flow transition on the surface obtained in S3; the mixture is continuously shaken and stirred for 30 minutes by a heated rotary mixer to compact and evenly distribute the hard abrasive on the surface of the thermoplastic polyurethane, so as to prepare thermoplastic polyurethane-based composite particles with hard abrasives evenly embedded on the surface; S5. Post-treatment of thermoplastic polyurethane-based soft elastic abrasive: collect the product prepared in S4 and place it at room temperature for 5 hours; then, pass the product through a 20# sieve and use a 40# sieve to collect the thermoplastic polyurethane-based soft elastic abrasive in the 40#-20# range, and obtain thermoplastic polyurethane-based soft elastic abrasive with a particle size range of 0.4-0.8 mm.
Citation Information
Patent Citations
Substrate treatment method for portion to be coated
CN101269479A
Method for producing metal mask for screen printing
CN101357525A
Method and device for manufacturing elastic abrasive method for blasting the elastic abrasive including method for recycling the elastic abrasive and device for blasting the elastic abrasive including device for recycling the elastic abrasive
CN104511844A
Elastic abrasive particle and manufacturing method thereof
CN105778861A
Anti-slip flooring material, method for manufacturing anti-slip flooring material, and method for constructing floor by using anti-slip flooring material
CN106030007A
Cited By
Hyperelastic composite abrasive material for jet polishing and preparation method and device of superelastic composite abrasive material
CN121652767A