A method for improving the uniformity of B element in alloy steel electroslag ingot

By refining the raw materials and inserting high-content B lines during the smelting of alloy steel electroslag ingots, and using protective atmosphere and B-Fe powder in electroslag remelting, the problem of unstable boron content is solved, and the Improve the uniformity of B element in electroslag ingots and improve the stability of the smelting process.

CN115838869BActive Publication Date: 2024-11-22SICHUAN JIANGYOU LIUHE STEAM TURBINE MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211557480.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-22
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

During the smelting of alloy steel electroslag ingots, the content of boron element is difficult to accurately control, resulting in unevenness and unstable performance of electroslag ingots. Especially in the production process of electroslag, the difference between the head and tail is large, which affects the whole The mass of the steel ingot.

Method used

By refining the alloy steel raw materials in one go, inserting high-content B lines, and using protective atmosphere and pre-slag materials, including B-Fe powder, during the electroslag remelting process, adjusting the electroslag slag system and atmosphere composition to ensure that Even distribution of B elements.

Benefits of technology

It significantly improves the uniformity of B element in the alloy steel electroslag ingot, reduces the difference in boron content between different batches, and improves the stability of the smelting process and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention discloses a method for improving the uniformity of the B element in an alloy steel electroslag ingot, which belongs to the field of special steel smelting. The method adopted by the present invention is: inserting a B wire into a primary smelting furnace and protecting the casting; adopting a protective electroslag remelting furnace during the electroslag process; adding B-Fe powder to the slag; adopting the method of the present invention to produce B-containing alloy steel products, and the B element content of the whole steel ingot is uniform. The method provided by the present invention solves the defects of the unstable B element content and large difference between different batches in the production process of the existing boron-containing alloy steel electroslag ingot. The B element content at both ends of the electroslag ingot obtained by the method of the present invention is not much different, and the difference in the boron content of the boron-containing electroslag ingots obtained by smelting between different batches is not much, and the uniformity of the boron element in the electroslag ingot has been greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy material preparation, to the smelting of special steel, and in particular to a method for improving the uniformity of B element in alloy steel electroslag ingot. Background Art

[0002] Boron can improve the hardenability of steel. Adding a trace amount of boron can double the hardenability of steel and strengthen the grain boundaries, significantly increasing the strength and hardness of steel. Adding a trace amount of boron to steel is equivalent to adding a certain proportion of Mn, Cr, and Ni. Therefore, replacing precious alloys such as Cr and Ni with a trace amount of boron can reduce the production cost of quenched and tempered steel.

[0003] However, since boron is extremely active, it is very easy to burn during high-temperature smelting, making it difficult to accurately control the boron content in alloy steel, resulting in unstable performance of boron-containing steel. In particular, during the electroslag production process, the difference between the head and the tail is more obvious, resulting in serious unevenness of the entire ingot, which makes it difficult to mass-smelt alloy steel electroslag ingots.

[0004] Therefore, how to solve the problem that the B element is not easy to be accurately controlled, the B content varies greatly, and the stability is poor during the smelting process of alloy steel electroslag ingots has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The purpose of the present invention is to solve the above technical problems, thereby providing a method for improving the uniformity of the B element in alloy steel electroslag ingots, so as to solve the problem that the B element content varies greatly and is difficult to control during the existing smelting process of B-containing electroslag ingots.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for improving the uniformity of B element in alloy steel electroslag ingot, wherein the element composition of the alloy steel includes, by weight percentage: C: 0.08-0.13, Mn: 0.35-0.65, Si≤0.10, S≤0.010, P≤0.015, Cr: 10.00-12.00, Ni: 0.30-0.70, Mo: 0.10-0.40, Co: 2.50-3.50, W: 2.40-3.00, V: 0.15-0.25, Nb: 0.05-0.12, N: 0.010-0.035, Al: ≤0.015, B: 0.01-0.025, and the balance is Fe;

[0008] The method comprises the following steps:

[0009] (1) performing a primary refining on the alloy steel raw material, inserting a B line during the primary refining process, wherein the B content in the B line is ≥ 20 wt%;

[0010] (2) After the first refining is completed, pouring is carried out in a protective atmosphere;

[0011] (3) The electroslag remelting is produced in a protective atmosphere electroslag remelting furnace, and the slag system of the electroslag remelting is: CaF2:MgO:Al2O3:Fe2O3=58:22:8:12;

[0012] (4) The electroslag slag material uses pre-melted slag and is mixed with 3-5% by weight of B-Fe powder.

[0013] Furthermore, the element composition of the alloy steel includes, by weight percentage, C: 0.10-0.12, Mn: 0.38-0.56, Si≤0.08, S≤0.010, P≤0.012, Cr: 10.50-11.80, Ni: 0.50-0.65, Mo: 0.20-0.35, Co: 2.70-3.20, W: 2.60-2.90, V: 0.18-0.23, Nb: 0.06-0.10, N: 0.015-0.030, Al: ≤0.012, B: 0.015-0.022, and the balance is Fe.

[0014] Furthermore, the element composition of the alloy steel includes, by weight percentage, C: 0.11, Mn: 0.44, Si≤0.05, S≤0.006, P≤0.010, Cr: 11.20, Ni: 0.58, Mo: 0.30, Co: 3.00, W: 2.75, V: 0.21, Nb: 0.08, N: 0.025, Al: ≤0.010, B: 0.020, and the balance is Fe.

[0015] Furthermore, the protective atmosphere is N2.

[0016] Furthermore, the weight ratio of B to Fe in the B-Fe powder is 3:1.

[0017] The beneficial effects of the present invention are as follows:

[0018] The method provided by the present invention solves the defects of unstable B element content and large difference between different batches in the existing production process of boron-containing alloy steel electroslag ingots. The B element content at both ends of the electroslag ingot obtained by the method of the present invention is not much different, and the boron content of the boron-containing electroslag ingots obtained by smelting from different batches is not much different, and the uniformity of the boron element in the electroslag ingot is greatly improved. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with embodiments.

[0020] Example 1

[0021] A method for improving the uniformity of B element in alloy steel electroslag ingot, comprising:

[0022] (1) performing a primary refining on the alloy steel raw material, inserting a B line during the primary refining process, wherein the B content in the B line is 20 wt%;

[0023] (2) After the first refining is completed, pouring is carried out in a protective atmosphere;

[0024] (3) The electroslag remelting is produced in a protective atmosphere electroslag remelting furnace, and the slag system of the electroslag remelting is: CaF2:MgO:Al2O3:Fe2O3=58:22:8:12;

[0025] (4) The electroslag slag material adopts pre-melted slag, and B-Fe powder accounting for 3% of the total weight of the slag is added.

[0026] The composition of the test steel used in the above smelting method is as follows:

[0027] Table 1 Chemical composition

[0028]

[0029]

[0030] Example 2

[0031] A method for improving the uniformity of B element in alloy steel electroslag ingot, comprising:

[0032] (1) performing a primary refining on the alloy steel raw material, inserting a B line during the primary refining process, wherein the B content in the B line is 22 wt %;

[0033] (2) After the first refining is completed, pouring is carried out in a protective atmosphere;

[0034] (3) The electroslag remelting is produced in a protective atmosphere electroslag remelting furnace, and the slag system of the electroslag remelting is: CaF2:MgO:Al2O3:Fe2O3=58:22:8:12;

[0035] (4) The electroslag slag material uses pre-melted slag and is mixed with 4% by weight of B-Fe powder.

[0036] The composition of the test steel used in the above smelting method is as follows:

[0037] Table 2 Chemical composition

[0038]

[0039] Example 3

[0040] A method for improving the uniformity of B element in alloy steel electroslag ingot, comprising:

[0041] (1) performing a primary refining on the alloy steel raw material, inserting a B line during the primary refining process, wherein the B content in the B line is 25 wt%;

[0042] (2) After the first refining is completed, pouring is carried out in a protective atmosphere;

[0043] (3) The electroslag remelting is produced in a protective atmosphere electroslag remelting furnace, and the slag system of the electroslag remelting is: CaF2:MgO:Al2O3:Fe2O3=58:22:8:12;

[0044] (4) The electroslag slag material uses pre-melted slag and is mixed with 5% by weight of B-Fe powder.

[0045] The composition of the test steel used in the above smelting method is as follows:

[0046] Table 3 Chemical composition

[0047]

[0048] Test Case

[0049] The B element content of different batches of alloy steel electroslag ingot products produced by the methods of Examples 1-3 was tested, the number of electroslag ingots produced in each batch was 100, the B element content of the ingot heads and ingot tails of the 100 electroslag ingots was tested, and the average value was taken. The results are shown in Table 4.

[0050] Table 4

[0051]

[0052] It can be seen from Table 4 above that the method of the present invention can obtain an alloy steel electroslag ingot with good uniformity of the B element, which effectively solves the problem of poor uniformity caused by the relatively active B element in the existing production process.

[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the uniformity of B element in alloy steel electroslag ingot, characterized in that: The element composition of the alloy steel is as follows by weight percentage: C: 0.11, Mn: 0.44, Si: 0.05, S: 0.006, P: 0.010, Cr: 11.20, Ni: 0.58, Mo: 0.30, Co: 3.00, W: 2.75, V: 0.21, Nb: 0.08, N: 0.025, Al: 0.010, B: 0.020, and the balance is Fe; The method comprises the following steps: (1) performing a primary refining on the alloy steel raw material, inserting a B line during the primary refining process, wherein the B content in the B line is 25 wt %; (2) After the first refining is completed, pouring is carried out in a N2 protective atmosphere; (3) The electroslag remelting is produced in a protective atmosphere electroslag remelting furnace, and the slag system of the electroslag remelting is: CaF2:MgO:Al2O3:Fe2O3=58:22:8:12; (4) The electroslag slag material adopts pre-melted slag and is mixed with 5% by weight of B-Fe powder, wherein the weight ratio of B to Fe in the B-Fe powder is 3:1.