Aluminum-doped cobalt carbonate, aluminum-doped cobalt tetroxide, preparation method, positive electrode material, lithium ion battery

Through the core-shell structure and preparation method of aluminum-doped cobalt tetroxide, the cracking problem of aluminum-doped cobalt carbonate during sintering is solved, and the performance and capacity retention rate of lithium-ion batteries are improved.

CN115849458BActive Publication Date: 2024-11-19GUANGXI CNGR NEW ENERGY SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211577863.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-19
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

In the prior art, cobalt aluminum-doped carbonate is prone to cracking when sintered into cobalt tetroxide, affecting the chemical performance of lithium batteries. The traditional coating method leads to inconsistent interface density and affecting battery performance.

Method used

The core-shell structure of aluminum-doped cobalt oxide is adopted, including aluminum-doped cobalt oxide core, intermediate layer and outer layer. By controlling the difference in porosity and density, a stable structure is formed to reduce the internal and external stress imbalance during sintering. The preparation method includes in the reactor The flow rate and pH value of cobalt aluminum solution and ammonium bicarbonate solution are regulated to form the target particle size and structure.

Benefits of technology

The stability of aluminum-doped cobalt carbonate during sintering is improved, the cracking of cobalt tetroxide is reduced, and the electrochemical performance and capacity retention rate of lithium-ion batteries are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115849458B_ABST
    Figure CN115849458B_ABST
Patent Text Reader

Abstract

The present application provides aluminum-doped cobalt carbonate, aluminum-doped cobalt tetroxide, preparation methods, positive electrode materials, and lithium-ion batteries, and relates to the field of new energy technology. The aluminum-doped cobalt carbonate includes an aluminum-doped cobalt carbonate core, an aluminum-doped cobalt carbonate middle layer, and an aluminum-doped cobalt carbonate outer layer. The difference in tap density, loose density, and porosity between the aluminum-doped cobalt carbonate core and the aluminum-doped cobalt carbonate outer layer is smaller, and the material is more stable during the subsequent sintering process of preparing cobalt tetroxide. The aluminum-doped cobalt carbonate middle layer of the present application has many pores and a loose structure. During the sintering process of cobalt tetroxide, it can be used as a buffer layer for the aluminum-doped cobalt carbonate core and the aluminum-doped cobalt carbonate outer layer, which can reduce the situation in which the sphere cracks due to uneven internal and external stresses during sintering into cobalt tetroxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new energy technology, and in particular to aluminum-doped cobalt carbonate, aluminum-doped cobalt tetroxide, preparation methods, positive electrode materials, and lithium-ion batteries. Background Art

[0002] Digital 3C devices currently often use lithium batteries as their power source. Charging voltage and capacity are important indicators of lithium batteries. The application of lithium batteries with lithium cobalt oxide as the positive electrode material is becoming more and more extensive. How to improve the working voltage and capacity of lithium cobalt oxide lithium batteries has become one of the huge challenges faced by positive electrode material manufacturers.

[0003] Cobalt carbonate can be sintered to obtain cobalt tetroxide. As a precursor of lithium cobalt oxide, the performance of cobalt tetroxide directly affects the performance of lithium cobalt oxide. In the prior art, in order to increase the capacity of lithium cobalt oxide, aluminum doping is often used. The higher the aluminum content, the greater the capacity improvement. However, correspondingly, aluminum is prone to enrichment, resulting in uneven distribution, affecting the capacity. Secondly, in the process of preparing aluminum-doped cobalt carbonate, the traditional coating method will form multiple interfaces. The density of cobalt carbonate on both sides of the interface is inconsistent, which will cause the cobalt carbonate to crack when sintered into cobalt tetroxide, thereby affecting the chemical properties of the battery. Summary of the invention

[0004] The purpose of the present application is to provide aluminum-doped cobalt carbonate and aluminum-doped cobalt tetroxide, aiming to solve the problem that the existing cobalt carbonate cracks when sintered into cobalt tetroxide, thereby affecting the chemical performance of the battery.

[0005] To achieve the above objectives, the present application provides an aluminum-doped cobalt oxide, wherein the aluminum-doped cobalt oxide has a core-shell structure and comprises:

[0006] An aluminum-doped cobalt oxide core, wherein the porosity of the aluminum-doped cobalt oxide core is 3% to 7%;

[0007] An aluminum-doped cobalt oxide intermediate layer, wherein the aluminum-doped cobalt oxide intermediate layer wraps the aluminum-doped cobalt oxide core, and the porosity of the aluminum-doped cobalt oxide intermediate layer is 15% to 25%;

[0008] An aluminum-doped cobalt oxide outer layer, wherein the aluminum-doped cobalt oxide outer layer encapsulates the aluminum-doped cobalt oxide middle layer, and the porosity of the aluminum-doped cobalt oxide outer layer is 10% to 20%;

[0009] The overall porosity of the aluminum-doped cobalt oxide is 10% to 20%.

[0010] Preferably, the aluminum-doped cobalt oxide satisfies at least one of the following characteristics E to J:

[0011] E. The aluminum content in aluminum-doped cobalt tetroxide is 0.5% to 0.8%;

[0012] F. The particle size D50 of aluminum-doped cobalt oxide is 15.0 to 20.0 μm;

[0013] G. The overall tap density of aluminum-doped cobalt oxide is 2.5 to 3.0 g / cm 3 ;

[0014] H. The overall bulk density of aluminum-doped cobalt oxide is 1.3 to 1.5 g / cm 3 ;

[0015] I. The specific surface area of ​​aluminum-doped cobalt oxide is 1.0 to 3.5 m 2 / g;

[0016] J. The 100-plane half-peak width in the XRD pattern of aluminum-doped cobalt oxide is 0.18-0.19.

[0017] Preferably, the aluminum-doped cobalt oxide core includes at least one of the following features a-b:

[0018] a. The diameter of the aluminum-doped cobalt oxide core is 8 to 12 μm;

[0019] b. The primary particles of the aluminum-doped cobalt oxide core are block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt oxide core are arranged in a disordered manner;

[0020] The aluminum-doped cobalt oxide intermediate layer includes at least one of the following features c to d:

[0021] c. The thickness of the aluminum-doped cobalt tetroxide intermediate layer encapsulating the aluminum-doped cobalt tetroxide core is 1 to 3 μm;

[0022] d. The primary particles of the aluminum-doped cobalt oxide intermediate layer are strip-shaped, and the strip-shaped primary particles of the aluminum-doped cobalt oxide intermediate layer are arranged in a disordered manner;

[0023] The aluminum-doped cobalt oxide outer layer includes at least one of the following features e to f:

[0024] e. The thickness of the aluminum-doped cobalt oxide outer layer wrapped with the aluminum-doped cobalt oxide middle layer is 1 to 5 μm;

[0025] f. The primary particles of the outer layer of aluminum-doped cobalt oxide are in the shape of strips, and the strip-shaped primary particles of the outer layer of aluminum-doped cobalt oxide are arranged radially from inside to outside.

[0026] The present application also provides an aluminum-doped cobalt carbonate, which has a core-shell structure and includes:

[0027] Aluminum carbonate-doped cobalt core, wherein the porosity of the aluminum carbonate-doped cobalt core is 1% to 5%;

[0028] A cobalt-aluminum carbonate-doped middle layer, wherein the cobalt-aluminum carbonate-doped middle layer wraps the cobalt-aluminum carbonate-doped inner core, and the porosity of the cobalt-aluminum carbonate-doped middle layer is 3% to 8%;

[0029] An outer layer of cobalt-doped aluminum carbonate, wherein the outer layer of cobalt-doped aluminum carbonate wraps the middle layer of cobalt-doped aluminum carbonate, and the porosity of the outer layer of cobalt-doped aluminum carbonate is 1% to 5%;

[0030] The overall porosity of the aluminum-doped cobalt carbonate is 2% to 5%.

[0031] Preferably, the aluminum-doped cobalt carbonate satisfies at least one of the following characteristics A to D:

[0032] A. The amount of aluminum in aluminum-doped cobalt carbonate is 0.3% to 0.6%;

[0033] B. The particle size D50 of aluminum-doped cobalt carbonate is 19.0 to 26.0 μm;

[0034] C. The overall tap density of cobalt carbonate doped with aluminum is 2.0 to 2.5 g / cm 3 ;

[0035] D. The overall bulk density of cobalt-aluminum carbonate is 1.5-2.0 g / cm 3 .

[0036] Preferably, the core of the aluminum-doped cobalt carbonate comprises at least one of the following features (1) to (4):

[0037] (1) The diameter of the core of cobalt aluminate is 14-16 μm;

[0038] (2) The primary particles of the aluminum-doped cobalt carbonate core are block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt carbonate core are arranged in a disordered manner;

[0039] (3) The tap density of the cobalt aluminum carbonate core is 2.0-2.3 g / cm 3 ;

[0040] (4) The bulk density of the cobalt-aluminum carbonate core is 1.4-1.9 g / cm 3 ;

[0041] The aluminum-doped cobalt carbonate intermediate layer includes at least one of the following features (5) to (6):

[0042] (5) The thickness of the aluminum-doped cobalt carbonate intermediate layer wrapping the aluminum-doped cobalt carbonate core is 1 to 3 μm;

[0043] (6) The primary particles of the aluminum-doped cobalt carbonate intermediate layer are in strip shape, and the strip-shaped primary particles of the aluminum-doped cobalt carbonate intermediate layer are arranged in a disordered manner;

[0044] The aluminum-doped cobalt carbonate outer layer includes at least one of the following features (7) to (8):

[0045] (7) The thickness of the aluminum-doped cobalt carbonate outer layer encapsulating the aluminum-doped cobalt carbonate middle layer is 2 to 6 μm;

[0046] (8) The primary particles of the outer layer of the cobalt carbonate doped with aluminum are in the shape of strips, and the strip-shaped primary particles of the outer layer of the cobalt carbonate doped with aluminum are arranged radially from inside to outside.

[0047] The present application also provides a method for preparing the aluminum-doped cobalt carbonate as described above, comprising:

[0048] Preparing seed crystals: introducing a cobalt aluminum solution and an ammonium bicarbonate solution into a first reaction kettle having a first base liquid added thereto, and reacting and growing to obtain seed crystals having a target particle size D50 of 14 to 16 μm;

[0049] Seed growth: Into the second reactor added with seed crystals and the second base liquid, cobalt aluminum solution and ammonium bicarbonate solution are introduced for the first growth. After the first growth is completed, the flow rate of the cobalt aluminum solution and the ammonium bicarbonate solution is adjusted to the flow rate of the seed crystal preparation process, and the second growth is carried out to obtain cobalt carbonate particles with a target particle size D50 of 19 to 26 μm.

[0050] Preferably, the preparation method of aluminum-doped cobalt carbonate includes at least one of the following features I to VII:

[0051] I. The concentration of ammonium bicarbonate in the first base solution is 40-70 g / L and the initial pH value is between 7.8-8.5;

[0052] II. The cobalt concentration in the cobalt-aluminum solution is 110-130 g / L and the aluminum concentration is 0.4-1.2 g / L;

[0053] III. The flow rate of the cobalt-aluminum solution introduced into the first reactor is 2.2-7.2% / h, and the flow rate of the ammonium bicarbonate solution is 6.6-20.0% / h;

[0054] IV. The pH of the reaction process in the first reactor is between 7.2±0.2;

[0055] V. The concentration of ammonium bicarbonate in the second base solution is 20-40 g / L and the initial pH value is between 7.5-8.0;

[0056] VI. During the first growth process, the flow rate of the cobalt aluminum solution introduced into the second reactor was 2.2-5.5% / h, the flow rate of the ammonium bicarbonate solution was 6.6-11.1% / h, and the particle size of the material increased by 1-3μm;

[0057] VII. The pH of the second growth reaction was 7.0±0.2.

[0058] The present application also provides a method for preparing aluminum-doped cobalt tetroxide, which is obtained by sintering the above-mentioned aluminum-doped cobalt carbonate.

[0059] The present application also provides a positive electrode material, the raw material of which includes the above-mentioned aluminum-doped cobalt tetroxide.

[0060] The present application also provides a lithium-ion battery, the positive electrode of which includes the positive electrode material mentioned above.

[0061] Compared with the prior art, the beneficial effects of this application include:

[0062] The aluminum-doped cobalt carbonate provided by the present application includes an aluminum-doped cobalt carbonate core, an aluminum-doped cobalt carbonate middle layer and an aluminum-doped cobalt carbonate outer layer. The difference in tap density, bulk density and porosity between the aluminum-doped cobalt carbonate core and the aluminum-doped cobalt carbonate outer layer is smaller, and the material is more stable in the subsequent sintering process of preparing cobalt tetroxide. The aluminum-doped cobalt carbonate middle layer of the present application has many pores and a loose structure. During the sintering process of cobalt tetroxide, it can be used as a buffer layer for the aluminum-doped cobalt carbonate core and the aluminum-doped cobalt carbonate outer layer, which can reduce the situation of cracking of the sphere caused by uneven internal and external stresses during sintering into cobalt tetroxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0064] Figure 1 This is a schematic diagram of the structure of aluminum-doped cobalt carbonate of the present application;

[0065] Figure 2 This is a scanning electron microscope morphology result diagram of the aluminum-doped cobalt carbonate of Example 1;

[0066] Figure 3 This is a scanning electron microscope morphology result of aluminum-doped cobalt tetroxide of Example 1;

[0067] Figure 4 The scanning electron microscope morphology result of the cross section of the aluminum-doped cobalt tetroxide of Example 1;

[0068] Figure 5 This is a scanning electron microscope morphology result of the cobalt carbonate doped with aluminum of Comparative Example 1;

[0069] Figure 6 This is a scanning electron microscope morphology result of aluminum-doped cobalt tetroxide of Comparative Example 1;

[0070] Figure 7 The scanning electron microscope morphology result of the cross section of the aluminum-doped cobalt tetroxide of Comparative Example 1;

[0071] Figure 8 The XRD patterns of cobalt tetroxide of Example 1 and Comparative Example 1 are shown in FIG.

[0072] Fig. 9 This is a surface scanning spectrum of the cobalt element of aluminum-doped cobalt tetroxide of Example 1;

[0073] Fig.10 This is a surface scanning spectrum of aluminum element of aluminum-doped cobalt tetroxide of Example 1;

[0074] Fig.11 The first charge capacity results of the lithium-ion batteries of the embodiments and comparative examples are shown;

[0075] Fig.12 The capacity retention rate results of the lithium ion batteries of the embodiments and comparative examples are shown;

[0076] Fig.13 The 0.1C rate test results of the lithium ion batteries of the embodiments and comparative examples are shown;

[0077] Fig.14 The 0.5C rate test results of the lithium ion batteries of the embodiments and comparative examples are shown;

[0078] Fig.15 This is a schematic diagram of the preparation method of aluminum-doped cobalt carbonate of the present application.

[0079] Reference numerals:

[0080] 100-cobalt-aluminum carbonate-doped inner core; 200-cobalt-aluminum carbonate-doped middle layer; 300-cobalt-aluminum carbonate-doped outer layer. DETAILED DESCRIPTION

[0081] As used herein:

[0082] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0083] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0084] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0085] In these examples, parts and percentages are by mass unless otherwise indicated.

[0086] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0087] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0088] Cobalt carbonate can be sintered to obtain cobalt tetroxide, which is the raw material for preparing lithium cobalt oxide positive electrode materials. Cobalt tetroxide and lithium source are calcined to obtain lithium cobalt oxide. The performance of cobalt tetroxide determines the performance of lithium cobalt oxide positive electrode materials, which is inherited. However, the performance of cobalt tetroxide is determined by cobalt carbonate. Therefore, the present application first provides an aluminum-doped cobalt carbonate, which is a core-shell structure, such as Figure 1 As shown, it includes: a cobalt aluminum carbonate doped core 100, a cobalt aluminum carbonate doped middle layer 200 and a cobalt aluminum carbonate doped outer layer 300.

[0089] Among them, the porosity of the cobalt aluminum carbonate core 100 is 1% to 5%, and the cobalt aluminum carbonate core 100 is relatively dense. The porosity can be, for example, 1%, 2%, 3%, 4% or 5%, or any value between 1% and 5%; the cobalt aluminum carbonate middle layer 200 wraps the cobalt aluminum carbonate core 100, and the porosity of the cobalt aluminum carbonate middle layer 200 is 3% to 8%, and the structure is relatively loose. The porosity can be, for example, 3%, 4%, 5%, 6%, 7% or 8%, or any value between 3% and 8%; the cobalt aluminum carbonate outer layer 300 wraps the cobalt aluminum carbonate middle layer 200, and the porosity of the cobalt aluminum carbonate outer layer 300 is 1% to 5%, and the cobalt aluminum carbonate outer layer 300 is relatively dense. The porosity can be, for example, 1%, 2%, 3%, 4% or 5%, or any value between 1% and 5%; and the overall porosity of the cobalt aluminum carbonate is 2% to 5%.

[0090] The tap density, bulk density and porosity of the cobalt carbonate core 100 and the aluminum-doped cobalt carbonate outer layer 200 provided in the present application are smaller, and the material is more stable in the subsequent sintering process of cobalt tetroxide. The aluminum-doped cobalt carbonate middle layer 200 of the cobalt carbonate of the present application has many pores and a loose structure. During the sintering process of cobalt tetroxide, it can be used as a buffer layer for the aluminum-doped cobalt carbonate core 100 and the aluminum-doped cobalt carbonate outer layer 300, which can reduce the situation of cracking of the sphere caused by uneven internal and external stresses during sintering into cobalt tetroxide.

[0091] The aluminum content of the aluminum-doped cobalt carbonate is 0.3% to 0.6%, for example, 0.32%, 0.4%, 0.45%, 0.48%, 0.5% or 0.6%, or any value between 0.3% and 0.6%.

[0092] The particle size D50 of the aluminum-doped cobalt carbonate is 19.0 to 26.0 μm, for example, 19.0 μm, 20.0 μm, 21.0 μm, 22.0 μm, 23.0 μm, 24.0 μm, 25.0 μm or 26.0 μm, or any value between 19.0 and 26.0 μm.

[0093] The overall tap density (TD) of the aluminum-doped cobalt carbonate is 2.0-2.5 g / cm 3 , for example, it can be 2.0 g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 , 2.3g / cm 3 , 2.4g / cm 3 or 2.5g / cm 3 , or 2.0~2.5g / cm 3 Any value in between.

[0094] The overall bulk density (AD) of the aluminum-doped cobalt carbonate is 1.5-2.0 g / cm 3 , for example, 1.5 g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 or 2.0g / cm 3 , or 1.5~2.0g / cm 3 Any value in between.

[0095] Among them, the diameter of the aluminum-doped cobalt carbonate core 100 is 14 to 16 μm, for example, it can be 14 μm, 15 μm or 16 μm, or any value between 14 and 16 μm; the primary particle shape of the aluminum-doped cobalt carbonate core 100 is block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt carbonate core are arranged in a disordered manner.

[0096] The tap density of the aluminum-doped cobalt carbonate core 100 is 2.0-2.3 g / cm 3 , for example, it can be 2.0 g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 or 2.3g / cm 3 , or 2.0~2.3g / cm 3 Any value in between.

[0097] The bulk density of the cobalt aluminate core 100 is 1.4-1.9 g / cm 3 , for example, 1.4 g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 or 1.9 g / cm 3 , or 1.4~1.9g / cm 3 Any value in between.

[0098] Among them, the thickness of the cobalt aluminum carbonate middle layer 200 wrapping the cobalt aluminum carbonate core 100 is 1 to 3 μm, for example, it can be 1 μm, 2 μm or 3 μm, or any value between 1 and 3 μm. Preferably, the thickness of the cobalt aluminum carbonate middle layer 200 wrapping the cobalt aluminum carbonate core 100 is 1 to 2 μm; wherein the thickness of the cobalt aluminum carbonate middle layer 200 wrapping the cobalt aluminum carbonate core 100 refers to the width of the cobalt aluminum carbonate middle layer 200 on the cross section of the cobalt aluminum carbonate.

[0099] The primary particles of the aluminum-doped cobalt carbonate intermediate layer 200 are in strip shape, and the strip-shaped primary particles of the aluminum-doped cobalt carbonate intermediate layer 200 are arranged in a disordered manner to form the aluminum-doped cobalt carbonate intermediate layer 200 with larger pores.

[0100] The thickness of the cobalt-aluminum carbonate outer layer 300 encapsulating the cobalt-aluminum carbonate middle layer 200 is 2 to 6 μm, for example, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm or 6 μm, or any value between 2 and 6 μm. Preferably, the thickness of the cobalt-aluminum carbonate outer layer 300 encapsulating the cobalt-aluminum carbonate middle layer 200 is 2 to 3 μm. The thickness of the cobalt-aluminum carbonate outer layer 300 encapsulating the cobalt-aluminum carbonate middle layer 200 refers to the width of the cobalt-aluminum carbonate outer layer 300 on the cross section of the cobalt-aluminum carbonate.

[0101] The primary particles of the outer layer 300 of aluminum-doped cobalt carbonate are in strip shape, and the strip primary particles of the outer layer 300 of aluminum-doped cobalt carbonate are arranged radially from inside to outside. The radial structure can effectively diffuse gas, and the structure can also effectively prevent the particles from breaking under continuous charging and discharging of the battery, thereby improving the battery capacity, cycle performance, safety, etc.

[0102] The present application also provides a method for preparing the aluminum-doped cobalt carbonate as described above, please refer to Fig.15 ,include:

[0103] S100: preparing seed crystals: introducing a cobalt aluminum solution and an ammonium bicarbonate solution into a first reaction kettle to which a first base liquid has been added, and performing reaction growth to obtain seed crystals having a target particle size D50 of 14 to 16 μm.

[0104] The concentration of ammonium bicarbonate in the first bottom liquid is 40-70 g / L, and the initial pH value is between 7.8-8.5; the concentration of ammonium bicarbonate in the first bottom liquid can be, for example, 40-50 g / L, or 50-70 g / L, or 40-60 g / L, and more specifically, can be 40 g / L, 45 g / L, 50 g / L, 55 g / L, 60 g / L, 65 g / L or 70 g / L. The first bottom liquid is obtained by adding ammonium bicarbonate solution and water into the first reaction kettle and mixing, and the concentration of the prepared ammonium bicarbonate solution is 150-250 g / L.

[0105] The cobalt-aluminum solution is obtained by mixing cobalt salt and aluminum salt dissolved in water, the cobalt concentration in the cobalt-aluminum solution is 110-130 g / L, for example, it can be 110 g / L, 115 g / L, 120 g / L, 125 g / L or 130 g / L, and the aluminum concentration in the cobalt-aluminum solution is 0.4-1.2 g / L, for example, it can be 0.4 g / L, 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L, 1.0 g / L, 1.1 g / L, 1.2 g / L or 1.3 g / L.

[0106] Wherein, the flow rate of the cobalt aluminum solution introduced into the first reactor is 2.2-7.2% / h, for example, it can be 2.2% / h, 3.0% / h, 3.5% / h, 4.3% / h, 5.2% / h, 6.0% / h, 6.7% / h or 7.2% / h, or any value between 2.2-7.2% / h; the flow rate of the ammonium bicarbonate solution is 6.6-20.0% / h, for example, it can be 6.6% / h, 7.0% / h, 8.0% / h, 9.0% / h, 10.0% / h, 11.0% / h, 15.0% / h or 20.0% / h, or any value between 6.6-20.0% / h.

[0107] The pH of the reaction process in the first reactor is between 7.2±0.2.

[0108] Among them, the seed particle size is 14-16μm.

[0109] After the seed crystals are obtained, a centrifuge, a squeeze dryer and other equipment are used to dehydrate the seed crystals to obtain a seed cobalt carbonate wet material.

[0110] S200: Seed growth: A cobalt aluminum solution and an ammonium bicarbonate solution are introduced into a second reaction kettle to which seeds and a second base liquid are added for the first growth. After the first growth is completed, the flow rates of the cobalt aluminum solution and the ammonium bicarbonate solution are adjusted to the flow rates of the seed preparation process, and a second growth is performed to obtain cobalt carbonate particles with a target particle size D50 of 19 to 26 μm.

[0111] The cobalt-aluminum solution is obtained by mixing cobalt salt and aluminum salt dissolved in water. The cobalt concentration in the cobalt-aluminum solution is 110-130 g / L, the aluminum concentration is 0.4-1.2 g / L, and the concentration of the ammonium bicarbonate solution is 150-250 g / L.

[0112] The second base liquid is obtained by mixing an ammonium bicarbonate solution with water, and the concentration of ammonium bicarbonate in the second base liquid is 20-40 g / L, for example, 20 g / L, 25 g / L, 30 g / L, 35 g / L or 40 g / L, and the initial pH value is between 7.5 and 8.0.

[0113] In the first growth process, the flow rate of the cobalt aluminum solution introduced into the second reactor is 2.2-5.5% / h, for example, 2.2% / h, 3.0% / h, 3.5% / h, 4.0% / h, 4.3% / h, 4.5% / h, 5.2% / h or 5.5% / h, or any value between 2.2-5.5% / h; the flow rate of the ammonium bicarbonate solution is 6.6-11.1% / h, for example, 6.6% / h, 7.0% / h, 8.0% / h, 8.5% / h, 9.0% / h, 9.5% / h, 10.0% / h or 11.0% / h, or any value between 6.6-11.1% / h. During the first growth process, the particle size increase of the material is controlled to be 1-3 μm. After the first growth is completed, an aluminum-doped cobalt carbonate intermediate layer is formed.

[0114] Among them, the reaction pH in the second growth process is 7.0±0.2, and the flow rates of the cobalt aluminum solution and the ammonium bicarbonate solution are adjusted to the flow rates of the cobalt aluminum solution and the ammonium bicarbonate solution in the seed crystal preparation process to ensure that the porosity, tap density and loose density of the inner core and the outer layer are less different.

[0115] The present application also provides an aluminum-doped cobalt tetroxide, which inherits the structure and performance of aluminum-doped cobalt carbonate. The aluminum-doped cobalt tetroxide is also a core-shell structure, including: an aluminum-doped cobalt tetroxide core, an aluminum-doped cobalt tetroxide middle layer and an aluminum-doped cobalt tetroxide outer layer. The aluminum-doped cobalt tetroxide core has a porosity of 3% to 7%, which is relatively dense. The porosity can be, for example, 3%, 4%, 5%, 6% or 7%, or any value between 3% and 7%. The aluminum-doped cobalt tetroxide middle layer wraps the aluminum-doped cobalt tetroxide core. The porosity of the aluminum-doped cobalt tetroxide middle layer is 15% to 25%, and the structure is relatively loose. The porosity can be, for example, 15%, 16%, 18%, 19%, 21% or 24%, or any value between 15% and 25%. The aluminum-doped cobalt oxide outer layer wraps the aluminum-doped cobalt oxide middle layer, and the porosity of the aluminum-doped cobalt oxide outer layer is 10% to 20%, for example, it can be 10%, 11%, 13%, 15%, 17% or 20%, or any value between 10% and 20%.

[0116] The overall porosity of the aluminum-doped cobalt oxide is 10% to 20%.

[0117] The aluminum content of the aluminum-doped cobalt tetroxide is 0.5% to 0.8%, for example, 0.5%, 0.6%, 0.7% or 0.8%, or any value between 0.5% and 0.8%.

[0118] The particle size D50 of the aluminum-doped cobalt oxide is 15.0-20.0 μm, for example, 15.0 μm, 16.0 μm, 17.0 μm, 18.0 μm, 19.0 μm or 20.0 μm, or any value between 15.0 and 20.0 μm.

[0119] The overall tap density of the aluminum-doped cobalt oxide is 2.5 to 3.0 g / cm 3 , for example, it can be 2.5 g / cm 3 , 2.6g / cm 3 , 2.7g / cm 3 , 2.8g / cm 3 , 2.9g / cm 3 or 3.0g / cm 3 , or 2.5~3.0g / cm 3 Any value in between.

[0120] The overall bulk density of the aluminum-doped cobalt oxide is 1.3-1.5 g / cm 3 , for example, 1.3 g / cm 3 , 1.4g / cm 3 or 1.5g / cm 3 , or 1.3~1.5g / cm 3 Any value in between.

[0121] The specific surface area of ​​the aluminum-doped cobalt oxide is 1.0 to 3.5 m 2 / g, for example, 1.0, 1.5m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g or 3.5m 2 / g, or 1.0~3.5m 2 Any value between / g.

[0122] The 100-plane half-peak width in the XRD spectrum of the aluminum-doped cobalt tetroxide is 0.18-0.19.

[0123] The diameter of the aluminum-doped cobalt oxide core is 8 to 12 μm, the primary particle shape is block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt oxide core are arranged in a disordered manner.

[0124] The thickness of the aluminum-doped cobalt oxide intermediate layer wrapping the aluminum-doped cobalt oxide core is 1 to 3 μm; the primary particles of the aluminum-doped cobalt oxide intermediate layer are strip-shaped, and the strip-shaped primary particles of the aluminum-doped cobalt oxide intermediate layer are arranged disorderly.

[0125] The thickness of the aluminum-doped cobalt oxide outer layer encapsulating the aluminum-doped cobalt oxide middle layer is 1 to 5 μm; preferably, the thickness of the aluminum-doped cobalt oxide outer layer encapsulating the aluminum-doped cobalt oxide middle layer is 1 to 2 μm. The primary particles of the aluminum-doped cobalt oxide outer layer are strip-shaped, and the strip-shaped primary particles of the aluminum-doped cobalt oxide outer layer are arranged radially from inside to outside.

[0126] The present application also provides a method for preparing aluminum-doped cobalt tetroxide, which is obtained by sintering the above-mentioned aluminum-doped cobalt carbonate.

[0127] The present application also provides a positive electrode material, the raw material of which includes the above-mentioned aluminum-doped cobalt tetroxide.

[0128] The present application also provides a lithium-ion battery positive electrode, the raw materials of which include the positive electrode material mentioned above.

[0129] The present application also provides a lithium-ion battery, comprising the above-mentioned lithium-ion battery positive electrode.

[0130] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0131] Example 1

[0132] The preparation method of aluminum-doped cobalt tetroxide of Example 1 comprises the following steps:

[0133] (1) Preparing a solution: dissolving cobalt chloride and aluminum sulfate in water to prepare a cobalt-aluminum solution having a cobalt concentration of 120 g / L and an aluminum concentration of 0.8 g / L; preparing an ammonium bicarbonate solution, controlling the concentration of the ammonium bicarbonate solution to be 140-160 g / L.

[0134] (2) Preparation of seed crystals: water and ammonium bicarbonate solution were added to the first reaction kettle as the first base liquid, the ammonium bicarbonate concentration in the first base liquid was controlled to be 40 g / L, and the initial pH value was controlled to be between 7.8 and 8.5. Then, the first reaction kettle was started to react at a speed of 80 r / min, and the flow rate of the cobalt aluminum solution introduced into the first reaction kettle during the reaction process was controlled to be 4.5% / h, the flow rate of the ammonium bicarbonate solution was controlled to be 15.0% / h, and the pH value of the reaction process was controlled to be between 7.2±0.2, and a precipitation reaction was carried out until the seed crystals grew to a target size D50 of 14.8 μm.

[0135] (3) Seed crystal centrifugation: The seed crystal slurry is dehydrated and dried using a centrifuge to obtain a wet seed crystal of cobalt carbonate.

[0136] (4) Seed growth: Put the seed into the empty second reactor, then add water and ammonium bicarbonate solution as the second bottom liquid, control the ammonium bicarbonate concentration in the second bottom liquid to 25g / L, and the initial pH value to be between 7.5-8.0. The second reactor starts the reaction at a speed of 80r / min, and the flow rate of the cobalt aluminum solution is controlled to be 3.0% / h and the flow rate of the ammonium bicarbonate solution is controlled to be 7.5% / h during the reaction process. The first growth is carried out, and the increase in the material particle size is controlled to be 2-3μm. After the first growth is completed, the flow rate of the cobalt aluminum solution is adjusted to 4.5% / h and the flow rate of the ammonium bicarbonate solution is adjusted to 15.0% / h, and the reaction pH value is controlled to be 7.0±0.2, and the second growth is carried out to finally obtain cobalt carbonate particles with a target particle size D50 of 20.5μm.

[0137] (5) Washing of cobalt carbonate: The cobalt carbonate slurry obtained by the reaction is washed using a centrifuge, and the temperature of the pure water is controlled at 40-50° C. After washing and dehydration, wet cobalt carbonate is obtained, and the scanning electron microscope morphology result is shown in the figure below. Figure 2 shown.

[0138] (6) Sintering: The wet cobalt carbonate material is sintered in a kiln at a high temperature of 350-800° C. to obtain the aluminum-doped cobalt tetroxide of Example 1, with a D50 of 17.2 μm. The scanning electron microscope morphology result is shown in the figure below: Figure 3 As shown, its cross-sectional view is as follows Figure 4 shown.

[0139] Example 2

[0140] The preparation method of aluminum-doped cobalt tetroxide of Example 2 comprises the following steps:

[0141] (1) Preparing a solution: dissolving cobalt chloride and aluminum sulfate in water to prepare a cobalt-aluminum solution having a cobalt concentration of 110-130 g / L and an aluminum concentration of 0.8-1.2 g / L; preparing an ammonium bicarbonate solution, controlling the concentration of the ammonium bicarbonate solution to be 140-160 g / L.

[0142] (2) Preparation of seed crystals: water and ammonium bicarbonate solution were added to the first reaction kettle as the first base liquid, the ammonium bicarbonate concentration in the first base liquid was controlled to be 50 g / L, and the initial pH value was controlled to be between 7.8 and 8.5. Then, the first reaction kettle was started to react at a speed of 80 r / min, and the flow rate of the cobalt aluminum solution introduced into the first reaction kettle during the reaction process was controlled to be 5.0% / h, the flow rate of the ammonium bicarbonate solution was controlled to be 16.0% / h, and the pH value of the reaction process was controlled to be between 7.2±0.2, and a precipitation reaction was carried out until the seed crystals grew to a target size D50 of 14.7 μm.

[0143] (3) Seed crystal centrifugation: The seed crystal slurry is dehydrated and dried using a centrifuge to obtain a wet seed crystal of cobalt carbonate.

[0144] (4) Seed growth: Put the seed into the empty second reactor, then add water and ammonium bicarbonate solution as the second bottom liquid, control the ammonium bicarbonate concentration in the second bottom liquid to 30g / L, and the initial pH value to be between 7.5-8.0. The second reactor starts the reaction at a speed of 80r / min, and the flow rate of the cobalt aluminum solution is controlled to be 4.0% / h and the flow rate of the ammonium bicarbonate solution is controlled to be 9.0% / h during the reaction process. The first growth is carried out, and the increase in the material particle size is controlled to be 2-3μm. After the first growth is completed, the flow rate of the cobalt aluminum solution is adjusted to 5.0% / h and the flow rate of the ammonium bicarbonate solution is adjusted to 16.0% / h, and the reaction pH value is controlled to be 7.0±0.2, and the second growth is carried out to finally obtain cobalt carbonate particles with a target particle size D50 of 20.6μm.

[0145] (5) Washing of cobalt carbonate: The cobalt carbonate slurry obtained by the reaction is washed using a centrifuge, and the temperature of pure water is controlled at 40-50° C. After washing and dehydration, wet cobalt carbonate is obtained.

[0146] (6) Sintering: The wet cobalt carbonate material is sintered in a kiln at a high temperature of 350-800° C. to obtain aluminum-doped cobalt tetroxide of Example 2, with a D50 of 17.3 μm.

[0147] Example 3

[0148] The preparation method of aluminum-doped cobalt tetroxide of Example 3 comprises the following steps:

[0149] (1) Preparing a solution: dissolving cobalt chloride and aluminum sulfate in water to prepare a cobalt-aluminum solution having a cobalt concentration of 110-130 g / L and an aluminum concentration of 0.8-1.2 g / L; preparing an ammonium bicarbonate solution, controlling the concentration of the ammonium bicarbonate solution to be 140-160 g / L.

[0150] (2) Preparation of seed crystals: water and ammonium bicarbonate solution were added to the first reaction kettle as the first base liquid, the ammonium bicarbonate concentration in the first base liquid was controlled to be 60 g / L, and the initial pH value was controlled to be between 7.8 and 8.5. Then, the first reaction kettle was started to react at a speed of 80 r / min, and the flow rate of the cobalt aluminum solution introduced into the first reaction kettle during the reaction process was controlled to be 5.5% / h, the flow rate of the ammonium bicarbonate solution was controlled to be 17.0% / h, and the pH value of the reaction process was controlled to be between 7.2±0.2, and a precipitation reaction was carried out until the seed crystals grew to a target size D50 of 14.9 μm.

[0151] (3) Seed crystal centrifugation: The seed crystal slurry is dehydrated and dried using a centrifuge to obtain a wet seed crystal of cobalt carbonate.

[0152] (4) Seed growth: Put the seed into the empty second reactor, then add water and ammonium bicarbonate solution as the second bottom liquid, control the ammonium bicarbonate concentration in the second bottom liquid to 35g / L, and the initial pH value to be between 7.5-8.0, start the reaction at 80r / min, control the flow rate of the cobalt aluminum solution to 5.0% / h and the flow rate of the ammonium bicarbonate solution to 10.0% / h during the reaction, carry out the first growth, and control the increase of the material particle size to 2-3μm. After the first growth is completed, adjust the flow rate of the cobalt aluminum solution to 5.5% / h and the flow rate of the ammonium bicarbonate solution to 17.0% / h, control the reaction pH value to 7.0±0.2, carry out the second growth, and finally obtain cobalt carbonate particles with a target particle size D50 of 20.4μm.

[0153] (5) Washing of cobalt carbonate: The cobalt carbonate slurry obtained by the reaction is washed using a centrifuge, and the temperature of pure water is controlled at 40-50° C. After washing and dehydration, wet cobalt carbonate is obtained.

[0154] (6) Sintering: The wet cobalt carbonate material is sintered in a kiln at a high temperature of 350-800° C. to obtain aluminum-doped cobalt oxide of Example 3, with a D50 of 17.0 μm.

[0155] Comparative Example 1

[0156] The preparation method of aluminum-doped cobalt tetroxide of Comparative Example 1 comprises the following steps:

[0157] (1) Solution preparation: Same as in Example 1.

[0158] (2) Preparation of seed crystals: Same as in Example 1.

[0159] (3) Seed centrifugation: same as in Example 1.

[0160] (4) Seed growth: The seed crystals were placed in an empty second reactor, and then water and ammonium bicarbonate solution were added as the second bottom liquid. The concentration of ammonium bicarbonate in the second bottom liquid was controlled to be 25 g / L, and the initial pH value was between 7.5 and 8.0. The second reactor was started to react at a speed of 80 r / min. The flow rate of the cobalt aluminum solution was controlled to be 4.5% / h and the flow rate of the ammonium bicarbonate solution was controlled to be 15.0% / h during the entire reaction process. The pH value of the reaction was controlled to be 7.0±0.2, and the growth was performed to finally obtain cobalt carbonate particles with a target particle size D50 of 20.5 μm. The scanning electron microscope morphology result is shown in the figure below. Figure 5 shown.

[0161] (5) Cobalt carbonate washing: same as in Example 1.

[0162] (6) Sintering: The aluminum-doped cobalt tetroxide of Comparative Example 1 was obtained in the same manner as in Example 1. The D50 was 17.2 μm. The scanning electron microscopy morphology result is shown in the figure below. Figure 6 As shown, it can be seen that the cobalt oxide of Comparative Example 1 has obvious cracks on its surface, and its cross-sectional view is as follows Figure 7 shown.

[0163] Comparative Example 2

[0164] The preparation method of aluminum-doped cobalt tetroxide of Comparative Example 2 comprises the following steps:

[0165] (1) Solution preparation: Same as in Example 1.

[0166] (2) Preparation of seed crystals: Same as in Example 1.

[0167] (3) Seed centrifugation: same as in Example 1.

[0168] (4) Seed growth: The seed crystals were placed in an empty second reactor, and then water and ammonium bicarbonate solution were added as the second bottom liquid. The concentration of ammonium bicarbonate in the second bottom liquid was controlled to be 25 g / L, and the initial pH value was between 7.5 and 8.0. The second reactor was started to react at a speed of 80 r / min. The flow rate of the cobalt aluminum solution was controlled to be 5% / h and the flow rate of the ammonium bicarbonate solution was controlled to be 16.0% / h during the entire reaction process. The reaction pH was controlled to be 7.0±0.2, and the growth was carried out to finally obtain cobalt carbonate particles with a target particle size D50 of 20.6 μm.

[0169] (5) Cobalt carbonate washing: same as in Example 1.

[0170] (6) Sintering: The same as in Example 1, i.e., the aluminum-doped cobalt tetroxide of Comparative Example 2 was obtained, and D50 was 17.3 μm.

[0171] The cobalt carbonate and cobalt tetroxide prepared in each embodiment and comparative example were subjected to relevant detection and analysis, and the tap density and bulk density of the inner core and the whole, and the porosity and width of the inner core, the middle layer and the outer layer were measured respectively. The measurement results of cobalt carbonate are shown in Table 1, and the measurement results of cobalt tetroxide are shown in Table 2.

[0172] Table 1 Indices of cobalt carbonate prepared in various embodiments and comparative examples

[0173]

[0174] Table 2 Indices of cobalt tetraoxide prepared in various embodiments and comparative examples

[0175]

[0176] According to Table 1 and Table 2, in Comparative Examples 1 and Comparative Examples 2, the flow rate of the cobalt-aluminum solution and the flow rate of the ammonium bicarbonate solution in the whole reaction remain unchanged during the seed growth process until the seed growth is completed, so the cobalt carbonate and cobalt tetroxide obtained are not three-layer structures, and there is no middle layer. Due to the inconsistent density of cobalt carbonate on both sides of the inner core and the outer layer, cobalt carbonate will cause cracking when sintered into cobalt tetroxide. The cobalt carbonate of the present application scheme includes an inner core, an intermediate layer and an outer layer, and the density of the inner core and the outer layer of cobalt carbonate is close, so as to avoid the inconsistent density of cobalt carbonate inside and outside during the coating process, resulting in cracking when finally sintered into cobalt tetroxide.

[0177] The difference in the tap density, bulk density and porosity of the cobalt carbonate of the embodiment of the present application is smaller, and the material is more stable in the subsequent preparation process; the middle layer of the cobalt carbonate of the embodiment has many pores and a loose structure. During the sintering process of cobalt tetroxide, it can be used as a buffer layer between the inner core and the outer layer, which can reduce the cracking of the sphere due to uneven internal and external stress during sintering into cobalt tetroxide. The outer layer has moderate pores and a radial structure; the radial structure can effectively diffuse gas, and the structure can also effectively prevent the battery from breaking particles under continuous charging and discharging, thereby improving the battery capacity, cycle performance, safety, etc.

[0178] Test example

[0179] 1. XRD patterns of cobalt oxide in Example 1 and Comparative Example 1

[0180] The XRD patterns of cobalt tetraoxide of Example 1 and Comparative Example 1 are as follows: Figure 8 As shown, according to Figure 8 It can be seen that the XRD diffraction peak of the cobalt oxide of Example 1 is consistent with the standard Co3O4 diffraction peak, and its 100-face half-peak width FWHM is 0.188, and the 100-face half-peak width FWHM of the cobalt oxide of Comparative Example 1 is 0.182. According to the Scherrer formula D=Kγ / (Bcosθ), B is the half-peak width of the sample diffraction peak, and D is the average thickness of the grain; the half-peak width of Example 1 is larger and the grains are smaller (consistent with the particle size comparison shown by SEM), which can improve the diffusion rate of lithium and improve the rate performance and cycle stability of the material.

[0181] 2. EDS-surface scan of cobalt tetroxide in Example 1

[0182] The surface of the cobalt oxide sample of Example 1 is scanned using a scanning electron microscope to obtain a surface scanning spectrum including the distribution of elements on the surface of the material. Fig. 9 and Fig.10 As shown, according to Fig. 9 and Fig.10 It can be seen that cobalt and aluminum elements are evenly distributed inside the cobalt oxide particles, which is beneficial to stabilizing the battery structure and improving the battery capacity and cycle performance.

[0183] 3. Electrochemical performance of lithium batteries prepared from cobalt tetroxide in the examples and comparative examples

[0184] The cobalt tetraoxide of Examples 1-3 and Comparative Examples 1-2 were sintered at a Li / Co mass ratio of 1.045 at 1050°C for 10 hours to prepare positive electrode materials, and finally half-cells were prepared. The electrochemical properties of the lithium batteries of the Examples and Comparative Examples were tested. The results are shown in Tables 3 and 4. Figures 11 to 14 shown.

[0185] According to Table 3 and Fig.11 It can be seen that the average first charge capacity of the embodiment is 3.82 mAh / g higher than that of the comparative example. Fig.12 It can be seen that the average value of the capacity retention rate of the embodiment is 3.2% higher than that of the comparative example; the 0.1C capacity test comparison result shows that the average value of the embodiment is 3.85mAh / g higher than that of the comparative example; the 0.5C capacity test comparison result shows that the average value of the embodiment is 9.22mAh / g higher than that of the comparative example; the 0.5C / 0.1C rate comparison result shows that the average value of the embodiment is 3.13% higher than that of the comparative example. This shows that the cobalt tetroxide obtained in the embodiment of the present application can improve the electrochemical performance of lithium-ion batteries.

[0186] Table 3 Electrochemical performance of lithium batteries obtained in various embodiments and comparative examples

[0187]

[0188] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0189] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. An aluminum-doped cobalt oxide, characterized in that: The aluminum-doped cobalt oxide is a core-shell structure, comprising: An aluminum-doped cobalt oxide core, wherein the aluminum-doped cobalt oxide core has a dense structure, a diameter of the aluminum-doped cobalt oxide core is 8 to 12 μm, and a porosity of 3% to 7%; An aluminum-doped cobalt oxide intermediate layer, wherein the aluminum-doped cobalt oxide intermediate layer wraps the aluminum-doped cobalt oxide core, the aluminum-doped cobalt oxide intermediate layer has a loose structure, the thickness of the aluminum-doped cobalt oxide intermediate layer wrapping the aluminum-doped cobalt oxide core is 1 to 3 μm, and the porosity of the aluminum-doped cobalt oxide intermediate layer is 16% to 25%; An aluminum-doped cobalt oxide outer layer, wherein the aluminum-doped cobalt oxide outer layer wraps the aluminum-doped cobalt oxide middle layer, the aluminum-doped cobalt oxide outer layer has a dense structure, the primary particles of the aluminum-doped cobalt oxide outer layer are strip-shaped, the primary particles of the aluminum-doped cobalt oxide outer layer are radially arranged from inside to outside, the thickness of the aluminum-doped cobalt oxide outer layer wrapping the aluminum-doped cobalt oxide middle layer is 1-5 μm, and the porosity of the aluminum-doped cobalt oxide outer layer is 10%-14%; The overall porosity of the aluminum-doped cobalt oxide is 10% to 20%.

2. The aluminum-doped cobalt tetroxide according to claim 1, characterized in that The aluminum-doped cobalt oxide satisfies at least one of the following characteristics E to J: E. The aluminum-doped cobalt tetroxide has an aluminum-doped content of 0.5% to 0.8%; F. The particle size D50 of the aluminum-doped cobalt oxide is 15.0-20.0 μm; G. The overall tap density of the aluminum-doped cobalt oxide is 2.5-3.0 g / cm³; H. The overall bulk density of the aluminum-doped cobalt oxide is 1.3-1.5 g / cm³; I. The specific surface area of ​​the aluminum-doped cobalt oxide is 1.0 to 3.5 m 2 / g; J. The 100-plane half-peak width in the XRD spectrum of the aluminum-doped cobalt oxide is 0.18-0.

19.

3. The aluminum-doped cobalt tetraoxide according to claim 1 or 2, characterized in that: The primary particles of the aluminum-doped cobalt oxide core are block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt oxide core are arranged in a disordered manner; The primary particles of the aluminum-doped cobalt oxide intermediate layer are in the shape of strips, and the strip-shaped primary particles of the aluminum-doped cobalt oxide intermediate layer are arranged in a disordered manner.

4. A cobalt carbonate doped with aluminum, characterized in that: The aluminum-doped cobalt carbonate is a core-shell structure, comprising: A cobalt-aluminum carbonate-doped core, wherein the cobalt-aluminum carbonate-doped core has a dense structure, a diameter of the cobalt-aluminum carbonate-doped core is 14-16 μm, and a porosity of the cobalt-aluminum carbonate-doped core is 1%-3%; An aluminum-doped cobalt carbonate intermediate layer, wherein the aluminum-doped cobalt carbonate intermediate layer wraps the aluminum-doped cobalt carbonate core, the aluminum-doped cobalt carbonate intermediate layer has a loose structure, the aluminum-doped cobalt carbonate intermediate layer wraps the aluminum-doped cobalt carbonate core to a thickness of 1 to 3 μm, and the aluminum-doped cobalt carbonate intermediate layer has a porosity of 5% to 8%; An outer layer of cobalt doped with aluminum carbonate, wherein the outer layer of cobalt doped with aluminum carbonate wraps the middle layer of cobalt doped with aluminum carbonate, the outer layer of cobalt doped with aluminum carbonate has a dense structure, the primary particles of the outer layer of cobalt doped with aluminum carbonate are in the shape of strips, the primary particles of the outer layer of cobalt doped with aluminum carbonate are arranged radially from inside to outside, the thickness of the outer layer of cobalt doped with aluminum carbonate wrapping the middle layer of cobalt doped with aluminum carbonate is 2-6 μm, and the porosity of the outer layer of cobalt doped with aluminum carbonate is 1%-3%; Wherein, the overall porosity of the aluminum-doped cobalt carbonate is 2% to 5%.

5. The aluminum-doped cobalt carbonate according to claim 4, characterized in that The aluminum-doped cobalt carbonate satisfies at least one of the following characteristics A to D: A. The aluminum content of the aluminum-doped cobalt carbonate is 0.3% to 0.6%; B. The particle size D50 of the aluminum-doped cobalt carbonate is 19.0-26.0 μm; C. The overall tap density of the aluminum-doped cobalt carbonate is 2.0-2.5 g / cm³; D. The overall bulk density of the aluminum-doped cobalt carbonate is 1.5-2.0 g / cm³.

6. The aluminum-doped cobalt carbonate according to claim 4 or 5, characterized in that: The kernel includes at least one of the following features (1) to (3): (1) The primary particles of the aluminum-doped cobalt carbonate core are block-shaped, and the block-shaped primary particles of the aluminum-doped cobalt carbonate core are arranged in a disordered manner; (2) The tap density of the aluminum-doped cobalt carbonate core is 2.0-2.3 g / cm³; (3) The bulk density of the aluminum-doped cobalt carbonate core is 1.4-1.9 g / cm³; The aluminum-doped cobalt carbonate intermediate layer includes the following features (4): (4) The primary particles of the aluminum-doped cobalt carbonate intermediate layer are in the shape of strips, and the strip-shaped primary particles of the aluminum-doped cobalt carbonate intermediate layer are arranged in a disordered manner.

7. A method for preparing aluminum-doped cobalt carbonate according to any one of claims 4 to 6, characterized in that: include: Preparing seed crystals: introducing a cobalt aluminum solution and an ammonium bicarbonate solution into a first reaction kettle having a first base liquid added thereto, and reacting and growing to obtain seed crystals having a target particle size D50 of 14 to 16 μm; Seed crystal growth: a cobalt-aluminum solution and an ammonium bicarbonate solution are introduced into a second reaction kettle to which the seed crystal and the second base liquid are added for the first growth. After the first growth is completed, the flow rates of the cobalt-aluminum solution and the ammonium bicarbonate solution are adjusted to the flow rates of the seed crystal preparation process, and a second growth is performed to obtain cobalt carbonate particles with a target particle size D50 of 19 to 26 μm.

8. The method for preparing aluminum-doped cobalt carbonate according to claim 7, characterized in that: The preparation method comprises at least one of the following features I to VII: I. the ammonium bicarbonate concentration in the first base solution is 40-70 g / L and the initial pH value is between 7.8-8.5; II. The cobalt concentration in the cobalt-aluminum solution is 110-130 g / L and the aluminum concentration is 0.4-1.2 g / L; III. The flow rate of the cobalt aluminum solution introduced into the first reactor is 2.2-7.2% / h, and the flow rate of the ammonium bicarbonate solution is 6.6-20.0% / h; IV. The pH of the reaction process in the first reactor is between 7.2±0.2; V. the concentration of ammonium bicarbonate in the second base solution is 20-40 g / L and the initial pH value is between 7.5-8.0; VI. During the first growth process, the flow rate of the cobalt-aluminum solution introduced into the second reactor was 2.2-5.5% / h, the flow rate of the ammonium bicarbonate solution was 6.6-11.1% / h, and the particle size of the material increased by 1-3 μm; VII. The pH of the second growth reaction was 7.0±0.

2.

9. A positive electrode material, characterized in that: The raw material comprises the aluminum-doped cobalt tetroxide as claimed in any one of claims 1 to 3.

10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery comprises the positive electrode material according to claim 9.