A high-performance waterproof and breathable fully flexible piezoelectric tactile sensor

The combination of PVDF nanofiber membrane and 2,6-diphenyl anthracene-OFET was prepared through electrospinning technology, which solved the challenges of flexible tactile sensors in terms of airtightness and wear comfort, and achieved high-performance waterproof and breathable. Suitable for long-term wear and real-time monitoring of human physiological signals.

CN115855323BActive Publication Date: 2024-12-06UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211479840.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-12-06
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

Existing flexible tactile sensors have defects in airtightness and wear comfort, making it difficult to have high sensitivity, waterproofness and breathability at the same time, and the material may cause discomfort and inflammation after long-term contact with the skin.

Method used

Electrospinning technology is used to prepare PVDF nanofiber membranes, combined with 2,6-diphenyl anthracene-OFET as signal amplification unit, forming a high-performance waterproof, breathable, fully flexible piezoelectric tactile sensor, using the natural hydrophobic characteristics of PVDF and the signal of OFET Amplification function enables flexibility, waterproof and breathable.

Benefits of technology

It realizes low energy consumption, high performance waterproof and breathable, suitable for long-term wear, can monitor human physiological signals in real time, and provides high-sensitivity piezoelectric stress sensors for human prosthetics and robotic arms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115855323B_ABST
    Figure CN115855323B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor. PVDF powder is dissolved in a mixed solution of N,N-dimethylformamide and acetone to prepare a PVDF solution; PVDF NM is obtained by electrostatic spinning; a PET film is used as a substrate; an aluminum film is deposited on the substrate to obtain a gate; a PMMA film is prepared on the gate to obtain a dielectric layer; 2,6-diphenylanthracene is thermally evaporated on the dielectric layer to obtain an active layer; a gold film is deposited on the active layer to obtain a source and drain electrode to obtain a DPA-OFET; the PVDF NM is connected to the DPA-OFET with a conductive tape and a wire to obtain a sensor. The present invention constructs a high-performance, energy-saving, waterproof and breathable fully flexible piezoelectric tactile sensor. It is used to prepare smart skin, has high pressure perception sensitivity, and will not cause discomfort after long-term contact with human skin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of flexible piezoelectric sensing technology, and in particular to a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor. Background Art

[0002] Pressure sensors, represented by tactile sensors, are one of the indispensable electronic components in cutting-edge fields such as human prostheses and robotic arms. Although great progress has been made in the development of such devices, it is still a huge challenge to obtain flexible tactile sensors that are highly sensitive, waterproof, and breathable.

[0003] Fortunately, with the continuous discovery and development of new materials, materials with outstanding piezoelectric properties and skin-friendly flexibility are being manufactured and used for pressure sensing, such as polarized polyvinylidene fluoride (PVDF) films, organic composite lead zirconate titanate (PZT), and ordered inorganic nanomaterials grown on flexible substrates such as zinc oxide (ZnO) and molybdenum disulfide (MoS2). However, when the above materials are used as electronic skin, they are generally prepared as organic piezoelectric films and inorganic nanostructures on rubber or dense plastic films as substrates. Therefore, they have defects in air tightness and are not suitable for people to wear for a long time. And after long-term contact with the skin, discomfort may occur, and even induce inflammation, swelling and itching. Therefore, it is very important and challenging to manufacture flexible devices with certain air and water vapor permeability.

[0004] Among the above materials, PVDF has natural hydrophobic properties, which can avoid the damage of external humid environment and wearer's sweat, thereby improving the stability and wearing comfort of the equipment. At the same time, as a functional polymer, PVDF has good processability like other conductive polymers, and can obtain porous and breathable structures similar to sponges, foams or aerogels by foaming, template synthesis, freeze drying and other methods. However, due to the limitations of these preparation methods, it is difficult to obtain β-PVDF with high electrical properties and porosity for the preparation of tactile sensors. Electrospinning, as a unique preparation technology for porous fiber membranes, has the advantages of simple manufacturing equipment, low spinning cost, a wide variety of spinning materials, controllable process, and the advantages of mechanical stretching and high-voltage electric field polarization in one step during electrospinning, and has become one of the main ways to effectively prepare nanofiber materials. However, due to the low piezoelectric strain constant of the material itself, the amount of charge generated under a small deformation force is limited, the force-electric conversion signal is weak, and it is easy to be buried in the noise, requiring high-precision instruments to measure. Therefore, the voltage amplification function of field effect transistors in electronic devices has been widely used. Summary of the invention

[0005] In view of the above-mentioned prior art, the purpose of the present invention is to provide a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor. The present invention combines the natural hydrophobic properties of PVDF nanofiber membrane (NM) with the signal amplification function of organic field effect transistors to construct a high-performance, energy-saving, waterproof, breathable fully flexible piezoelectric tactile sensor. It is used to prepare smart skin and will not cause discomfort after long-term contact with human skin.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] The first aspect of the present invention provides a high-performance waterproof, breathable and fully flexible piezoelectric tactile sensor, which includes a waterproof and breathable membrane and an organic field effect transistor connected thereto; the waterproof and breathable membrane is a PVDF nanofiber membrane made by electrospinning PVDF; the organic field effect transistor is 2,6-diphenylanthracene-OFET; the PVDF nanofiber membrane is used as a piezoelectric signal generating unit, and the 2,6-diphenylanthracene-OFET is used as a signal amplifying unit, conductive tapes are respectively attached to the two sides of the piezoelectric signal generating unit, the conductive tapes are connected to wires, and the two sides of the piezoelectric signal generating unit are respectively connected to the gate and source electrodes of the 2,6-diphenylanthracene-OFET by using the wires to form a closed loop.

[0008] Preferably, it is prepared by the following method:

[0009] (1) dissolving PVDF powder in a mixed solution of N,N-dimethylformamide and acetone to prepare a PVDF solution; performing high-voltage stretching polarization by electrospinning to obtain a polarized PVDF nanofiber membrane;

[0010] (2) Pre-cleaning the PET film, drying it with nitrogen, and then plasma cleaning it in an oxygen environment to obtain a substrate; depositing an aluminum film on the substrate to obtain a gate; spin-coating a PMMA solution on the gate to form a PMMA film, and then air-drying and evaporating the solvent to obtain a dielectric layer; thermally evaporating 2,6-diphenylanthracene on the dielectric layer to obtain an active layer; using a rectangular copper mesh as a mask, depositing a gold film on the active layer to obtain source and drain electrodes, thereby obtaining a DPA-OFET;

[0011] (3) Using PVDF NM as the piezoelectric signal generating unit and OFET as the signal amplifying unit, the two sides of the piezoelectric signal generating unit are connected to the gate and source electrodes of OFET respectively with conductive tape and wire to form a closed loop, thereby obtaining a high-performance waterproof, breathable and fully flexible piezoelectric tactile sensor.

[0012] Preferably, the concentration of the PVDF solution is 10wt%, the volume ratio of the N,N-dimethylformamide and acetone is 3:2; the diameter of the PVDF nanofibers in the PVDF nanofiber membrane is 400nm-600nm; and the contact angle of the PVDF nanofiber membrane is 125.43°.

[0013] Preferably, in step (1), the electrospinning process is: transferring the PVDF solution into a syringe, placing it in an electrospinning machine, performing high-voltage stretching polarization, laying a layer of aluminum foil to receive the polarized nanofiber membrane; and then ventilating and drying the nanofiber membrane received on the aluminum foil to evaporate the solvent.

[0014] Preferably, the voltage of the electrospinning is 20 kV, the needle tube pushing speed is 1.7 ml / h, and the distance between the needle tip and the aluminum foil is 15 cm; the temperature of the ventilation drying is 60° C. and the time is 2 h.

[0015] Preferably, in step (2), the pre-cleaning is to ultrasonically clean the PET film with deionized water, acetone and isopropanol in sequence.

[0016] Preferably, in step (2), the thickness of the aluminum film is 100 nm; the thickness of the PMMA film is 300 nm; the thickness of the 2,6-diphenylanthracene is 50 nm; and the thickness of the gold film is 50 nm.

[0017] Preferably, in step (2), the deposition rate is The concentration of the PMMA solution was 10 mg / ml, and the spin coating rate was 1000 rpm; the DPA deposition rate was The Au deposition rate is

[0018] Preferably, the minimum detection limit of the high-performance waterproof and breathable fully flexible piezoelectric tactile sensor is 48.54Pa and the sensitivity is 7.94KPa -1 .

[0019] The second aspect of the present invention provides the use of the above-mentioned high-performance waterproof, breathable and fully flexible piezoelectric tactile sensor in the preparation of intelligent electronic skin.

[0020] Beneficial effects of the present invention:

[0021] (1) The present invention combines the natural hydrophobic properties of PVDF with advanced electrospinning technology to obtain a piezoelectric film with interconnected fibers, thereby achieving flexibility, waterproofness and breathability of the sensor.

[0022] (2) Research on the device of the present invention, under the guidance of piezoelectric electronics, PVDF NM and OFET capacitive coupling construct a low-energy consumption, high-performance waterproof and breathable flexible tactile sensor, laying the foundation for the next step of OFET amplification of piezoelectric stress sensors and tactile sensor chips. At the same time, the arrangement pattern of organic small molecule materials and the performance of polymer stacking are deeply characterized to guide the synthesis of large-area semiconductor layers.

[0023] (3) The present invention studies the influence of piezoelectric discharge on the transport performance of OFET semiconductors. By regulating the gate voltage of OFET, the amplification mechanism and law of the PVDF NM force-electric coupling effect are mastered. Further in-depth research is conducted on the pressure test limit, sensitivity, etc. to achieve real-time monitoring of human physiological signals. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The schematic diagram of the structure of a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor based on the coupling of DPA-OFET and PVDF NM.

[0025] As shown in the figure, 1. substrate, 2. gate, 3. dielectric layer, 4. active layer, 5. source and drain electrodes, 6. wires, 7. PVDFNM, and 8. conductive tape.

[0026] Figure 2 The SEM photos of PVDF NM and the statistical diagram of fiber diameter distribution;

[0027] Figure 3 The SEM photos and contact angle test diagrams of PVDF NM;

[0028] Figure 4 This is a photo of the air and water permeability experiment of PVDF NM;

[0029] Figure 5 This is a graph showing the mass change of the remaining water in the vial during the ten-day air and water permeability experiment of PVDF NM;

[0030] Figure 6 This is the waterproof test diagram of PVDF NM;

[0031] Figure 7 is the transfer characteristic curve of DPA-OFET;

[0032] Figure 8 is the transfer characteristic curve of DPA-OFET at different gate voltages;

[0033] Fig. 9 Output characteristics of DPA-OFET in the linear region;

[0034] Fig.10Output characteristics of DPA-OFET in the saturation region;

[0035] Fig.11 The output curve of PVDF-OFET-PZTS under different mass weights;

[0036] Fig.12 It is a linear simulation of the experimental value of the output curve of the high-performance waterproof and breathable fully flexible piezoelectric tactile sensor of the present invention under the action of different mass weights;

[0037] Fig.13 The actual photographs of the present invention when the finger bending angles are 0°, 5°, 30°, 60°, and 90°;

[0038] Fig.14 is the output curve of the device when the finger is bent at an angle according to the present invention;

[0039] Fig.15 This is the output curve of the device when the present invention tests the wrist pulse;

[0040] Fig.16 The output curve of the device when saying "Hi" at different volume levels is tested for the present invention;

[0041] Fig.17 The output curve of the device when testing walking and running for the present invention;

[0042] Fig.18 Schematic diagram of PVDF-OFET-PZTS when (a) mechanical force is applied and (b) mechanical force is released;

[0043] Fig.19 The output curve of pentacene OFET-PZTS under different mass weights;

[0044] Fig. 20 Linear simulation of the experimental values ​​of the output curve of pentacene OFET-PZTS under different mass weights. DETAILED DESCRIPTION

[0045] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0046] As described in the background technology, materials with outstanding piezoelectric properties and skin-fitting flexibility are generally used as electronic skins by preparing organic piezoelectric films and inorganic nanostructures on rubber or dense plastic films as substrates. It has defects in air tightness and is not suitable for people to wear for a long time. And it may cause discomfort after long-term contact with the skin, and even induce inflammation, swelling and itching. Although PVDF material can be used as a breathable material, its piezoelectric strain constant is low, the amount of charge generated under a small deformation force is limited, and the force-to-electricity conversion signal is weak and easily buried in the noise.

[0047] Based on this, the present invention provides a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor. The present invention uses PVDF with natural hydrophobic properties to prepare β-PVDF NM with high electrical performance and porosity through electrospinning for preparing waterproof and breathable flexible tactile sensors. The PVDF NM obtained by the present invention through electrospinning technology has a PVDF nanofiber diameter distribution between 400nm-600nm. The natural hydrophobicity of PVDF is combined with thousands of micropores in the PVDF nanofiber membrane, giving the device excellent waterproofness and breathability. At the same time, the interconnected structure between the fibers makes the obtained membrane have a wide deformation limit and a fast response time, making the device super flexible. When preparing OFET, the dielectric constant of PMMA is equivalent to that of silicon dioxide. The 30nm thick PMMA film can effectively insulate the gate voltage and induce changes in channel carriers, thereby reducing the leakage current. The transmission of carriers is mainly concentrated in several molecular layers between the active layer DPA and the dielectric layer PMMA. The 50nm active layer DPA film can be highly crystallized into a thin film and can also make the source and drain electrode carriers better injected and transmitted. In order to reduce the impact of electrode size on the test, a mask with large-sized electrodes and channels was prepared using ultraviolet laser engraving technology. Finally, the PVDF NM and DPA-OFET are combined together by conductive tape and wires. Figure 1 shown.

[0048] By capacitively coupling the functional material to the sensitive film or microstructure, a favorable electrical response is accompanied by external pressure or tension, or even occurs simultaneously under both stimuli. In the present invention, since DPA is a typical P-type semiconductor, the majority carriers in the channel when the DPA-OFET is working are holes. When pressure is applied, the PVDF NM is deformed, and the internal electric dipole moment shortens due to compression. To resist this change, equal amounts of positive and negative charges are generated on the relative surfaces of the material, which manifests as a positive voltage. This voltage acts as the gate voltage in the DPA-OFET. At this time, holes accumulate at the interface between the gate and the dielectric layer, thereby inducing additional electrons in the conductive channel of the DPA active layer. The electrons recombine with the majority carrier holes in the channel, resulting in a current I DSReduce, such as Fig.18 a; on the contrary, when the pressure is released, the PVDF NM quickly recovers its shape, and the generated polarization voltage changes from positive voltage to negative voltage. This causes the interface between the gate and the dielectric layer to accumulate electrons, thereby inducing additional holes in the channel, resulting in a current I DS The increase, such as Fig.18 When in use, the PVDF NM is attached to the human skin, thereby realizing the high sensitivity of the high-performance waterproof and breathable fully flexible piezoelectric tactile sensor to pressure, while also being waterproof and breathable.

[0049] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.

[0050] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.

[0051] Example

[0052] (1) Dissolve PVDF powder in a mixed solution of N,N-dimethylformamide and acetone to prepare a 10wt% PVDF solution (wherein the volume ratio of DMF to acetone is 3:2). After the solute is completely dissolved and there are no bubbles in the solution, use a syringe as a carrier to place the solution into the electrospinning machine. Set the following parameters: voltage 20KV, needle tube push speed 1.7ml / h, and the distance between the needle tip and the receiving roller is 15cm. Place a layer of aluminum foil on the receiver to receive the polarized PVDF nanofibers. After 5 hours, place the fiber membrane received on the aluminum foil in a ventilated environment at 60℃ and dry for 2 hours to evaporate the solvent, completing the preparation of waterproof and breathable flexible PVDF NM, and cut the PVDF NM into a size of 3cm×3cm as a piezoelectric signal generating unit for standby use;

[0053] (2) Experimental grade polyethylene terephthalate (PET) film was ultrasonically cleaned with deionized water, acetone and isopropanol for 5 min, with an ultrasonic power of 40 W, a temperature of 25°C and a time of 10 min. Then it was dried under nitrogen. Then it was plasma cleaned in an oxygen environment for 10 min, with a plasma cleaning power of 100 W, a temperature of 25°C and a time of 10 min to complete the cleaning of the substrate. The cleaned PET substrate was placed in a metal vacuum coating apparatus. A 100nm thick Al was thermally evaporated at a rate of 1000rpm as the gate electrode; then a 10mg / ml PMMA solution was prepared, and a 300nm thick PMMA film was formed on the aluminum electrode using a coating machine at a rate of 1000rpm, and then treated in a vacuum drying oven at 100℃ for 2h as the dielectric layer of the device; then an organic vacuum coating instrument was used to coat the PMMA film with a temperature of 100℃. The organic small molecule material DPA with a thickness of 50nm was thermally evaporated at a rate of 1000 nm to form an active layer; then a rectangular copper mesh (length 10mm, width 2mm, channel width 1mm) was used as a mask to cover the DPA film, and a metal vacuum coating apparatus was used again to A 50nm thick Au film was thermally evaporated at a rate of 1000 nm to obtain source and drain electrodes, thus completing the construction of DPA-OFET.

[0054] (3) Using PVDF NM as a piezoelectric signal generating unit and DPA-OFET as a signal amplifying unit, the two sides of PVDF NM were connected to the gate and source electrodes of OFET respectively using conductive tape (silver glue) and copper wire to form a closed loop, thus preparing a waterproof and breathable fully flexible tactile sensor based on piezoelectric coupling of PVDF NM and DPA-OFET (PVDF-OFET-PZTS), as shown in Figure 3. Figure 1 shown.

[0055] Comparative Example

[0056] (1) Preparation of waterproof and breathable flexible PVDF NM is the same as step (1) of Example;

[0057] (2) An experimental grade polyethylene terephthalate (PET) film was ultrasonically cleaned with deionized water, acetone, and isopropanol for 5 min, dried under nitrogen, and plasma cleaned in an oxygen environment for 10 min to complete the cleaning of the substrate; the cleaned PET substrate was placed in a metal vacuum coater. A 100nm thick Al was thermally evaporated at a rate of 1000rpm as the gate electrode; then a 10mg / ml PMMA solution was prepared, and a 300nm thick PMMA film was formed on the aluminum electrode using a coating machine at a rate of 1000rpm, and then treated in a vacuum drying oven at 100℃ for 2h as the dielectric layer of the device; then an organic vacuum coating instrument was used to coat the PMMA film with a temperature of 100℃. The organic small molecule material pentacene with a thickness of 50nm was thermally evaporated at a rate of 1000 nm to form an active layer; then a rectangular copper mesh (length 10mm, width 2mm, channel width 1mm) was used as a mask to cover the DPA film, and a metal vacuum coater was used again to coat the DPA film. A 50nm thick Au film was thermally evaporated at a rate of 1.50 to obtain source and drain electrodes, completing the construction of pentacene-OFET.

[0058] (3) The connection between PVDF NM and pentacene-OFET is the same as step (3) of the embodiment to prepare a waterproof, breathable, fully flexible tactile sensor (OFET-PZTS) based on piezoelectric coupling of PVDF NM and pentacene-OFET.

[0059] Test example

[0060] (1) The film quality of PVDF NM was detected by SEM and the diameter distribution of the fibers was statistically analyzed. The hydrophilicity and hydrophobicity of PVDF NM were detected by contact angle test. Figure 2 , 3 Next, the water vapor permeability of PVDF NM was examined, as shown in Figure 4 , 5 As shown, the amount of water remaining in five bottles containing 5 g of ultrapure water at room temperature for ten days was recorded (the five bottles were treated as follows: open, covered with a PET film, covered with a PDMS film, covered with a commercially available PVDF film, and covered with a PVDF NM); finally, the waterproofness of the PVDF NM was tested by dripping water on it, as shown in FIG. Figure 6 shown.

[0061] (2) The electrical properties of the DPA-OFET prepared in step (2) of Example 1 were tested using a platform built by a probe station EPS150TRIAX and a semiconductor test analyzer 4200SCS. Three probes were used to connect the source, drain and gate electrodes of the device respectively. GS The range is -80V-10V, V DS = -60V, the transfer characteristic curve, transmission characteristic curve, linear region and saturation region of the device are obtained. Figure 7-10 , and the mobility of the device was obtained to be 3.28cm 2 V -1 s -1 , the on / off ratio is 10 6 -10 7 ;

[0062] (3) Next, the electrical properties of the PVDF-DPA-OFET-PZTS prepared in step (3) of the example and the PVDF-pentacene OFET-PZTS prepared in the comparative example were tested. At this time, V GS = 0V, the sensor is obtained under the condition that the voltage is provided by PVDF NM under the force of weights of different masses (0g, 10g, 20g, 50g, 100g, 200g) (such as Fig.11 , 12 ) The minimum detection limit of the sensor of the embodiment is 48.54Pa and the sensitivity is 7.94KPa -1 PVDF-OFET-PZTS detects different finger bending angles (0°, 5°, 30°, 60° and 90°), pulse beats, vocal cord vibrations and walking signals (such as Figure 13-17 The output curve of the comparative sensor under different mass weights is shown in Fig.19 The linear simulation of the experimental output curve of pentacene OFET-PZTS with different mass weights is shown in Fig. 20The detection limit of the comparative sensor is 117.96Pa and the sensitivity is 4.13KPa. -1 DPA is a typical P-type organic semiconductor small molecule anthracene material, which is integrated with photoelectricity. Large-area high-mobility thin films can be obtained using a simple vacuum evaporation method. The mobility of pentacene OFETs obtained using the same construction method is 2.01×10 -2 cm 2 V -1 s -1 , while the mobility of DPA-OFET is 3.28cm 2 V -1 s -1 , which is 100 times that of pentacene OFET, indicating that PVDF NM and DPA-OFET are more conducive to signal transmission and amplification, and are beneficial to improving the accuracy of signal detection.

[0063] According to the above curve, under the guidance of piezoelectric electronics, when the PVDF-OFET-PZTS prepared in the embodiment works, various physiological signals stimulate the PVDF NM to produce current changes, and the current enters the gate of the DPA-OFET, and the gate voltage V GS To control the channel current I DS The PVDF NM and DPA-OFET capacitive coupling amplifies the pressure signal. The waterproof and breathable flexible piezoelectric sensor of the present invention can contribute to the development of artificial intelligence and biomedical wearable fields such as human prostheses and robot arms in the future.

[0064] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. Application of a high-performance waterproof and breathable fully flexible piezoelectric tactile sensor in improving the sensitive perception of pressure, characterized in that: The high-performance waterproof, breathable and fully flexible piezoelectric tactile sensor includes a waterproof and breathable membrane and an organic field effect transistor connected thereto; the waterproof and breathable membrane is a PVDF nanofiber membrane made of PVDF by electrospinning; the organic field effect transistor is 2, 6-diphenylanthracene-OFET; the PVDF nanofiber membrane is used as a piezoelectric signal generating unit, and the 2, 6-diphenylanthracene-OFET is used as a signal amplification unit, and conductive tapes are respectively attached to the two sides of the piezoelectric signal generating unit, and the conductive tapes are connected to the wires, and the two sides of the piezoelectric signal generating unit are respectively connected to the gate and source electrodes of the 2, 6-diphenylanthracene-OFET by the wires to form a closed loop; the minimum detection limit of the high-performance waterproof, breathable and fully flexible piezoelectric tactile sensor is 48.54 Pa, and the sensitivity is 7.94 Kpa -1 ; The high-performance waterproof and breathable fully flexible piezoelectric tactile sensor is prepared by the following method: (1) PVDF powder was dissolved in a mixed solution of N, N-dimethylformamide and acetone to prepare a 10 wt% PVDF solution, with a volume ratio of DMF to acetone of 3:

2. After the solute was completely dissolved and there were no bubbles in the solution, the solution was placed into an electrospinning machine using a syringe as a carrier, and the following parameters were set: voltage 20 KV, needle tube push speed 1.7 ml / h, and a distance of 15 cm between the needle tip and the receiving roller. A layer of aluminum foil was placed on the receiver to receive the polarized PVDF nanofibers. After 5 hours, the fiber membrane received on the aluminum foil was placed in a ventilated environment at 60 °C and dried for 2 hours to evaporate the solvent, completing the preparation of waterproof and breathable flexible PVDF NM. The PVDF NM was cut into 3 cm × 3 cm pieces as a piezoelectric signal generating unit for standby use. (2) An experimental grade polyethylene terephthalate (PET) film was ultrasonically cleaned with deionized water, acetone, and isopropanol for 5 min at an ultrasonic power of 40 W, a temperature of 25 °C, and a time of 10 min, and then dried under nitrogen. The film was then plasma cleaned in an oxygen environment for 10 min at a plasma cleaning power of 100 W, a temperature of 25 °C, and a time of 10 min to complete the cleaning of the substrate. The cleaned PET substrate was placed in a metal vacuum coater and the film was coated with a 0.1 Å s -1 100 nm thick Al was thermally evaporated at a rate of 100 rpm as the gate electrode; then 10 mg / ml PMMA solution was prepared, and a 300 nm thick PMMA film was formed on the aluminum electrode using a coater at a rate of 1000 rpm, and then treated in a vacuum oven at 100 °C for 2 h as the dielectric layer of the device; then an organic vacuum coater was used at a rate of 0.05 Å s -1 A 50 nm thick organic small molecule material DPA was thermally evaporated at a rate of 1.5 Å to form an active layer. Next, a rectangular copper mesh with a length of 10 mm, a width of 2 mm, and a channel width of 1 mm was used as a mask to cover the DPA film. A metal vacuum coating apparatus was used again at a rate of 0.5 Å s -1 A 50 nm thick Au film was thermally evaporated at a rate of 100 nm to obtain source and drain electrodes, thus completing the construction of DPA-OFET. (3) Using PVDF NM as the piezoelectric signal generating unit and DPA-OFET as the signal amplifying unit, the two sides of PVDF NM were connected to the gate and source electrodes of OFET respectively using conductive silver glue and copper wire to form a closed loop, thus preparing a waterproof, breathable and fully flexible tactile sensor based on piezoelectric coupling of PVDF NM and DPA-OFET.