A graphene aerogel with stable structure and high elasticity and preparation method thereof
Through directional freezing and thermal reduction processes, graphene aerogels with high elasticity and structural stability were prepared, which solved the stability and strength of graphene aerogel materials in the prior art, and was suitable for a variety of high-performance applications.
Patent Information
- Application Number
- CN202110984068.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-25
AI Technical Summary
The existing graphene aerogel preparation methods are complex and the materials have problems such as unstable structural, low strength, and weak elasticity, which hinder its further application in energy storage, sensing, catalysis and other fields.
Using a special directional freezing method and thermal reduction process, a graphene aerogel with a radial orientation structure is formed by centripetal freezing, and graphene oxide aerogel is prepared using copper molds and a low-temperature environment, and high-temperature heating is carried out in an inert atmosphere. Reduction to obtain graphene aerogel with high elasticity and structural stability.
It has achieved high elasticity and structural stability of graphene aerogel, high porosity, low density and low thermal conductivity. It is suitable for catalysis and sensor fields, and has a simple process and is environmentally friendly.
Smart Images

Figure CN115893391B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a graphene aerogel with stable structure and high elasticity and a preparation method thereof, and belongs to the field of nano materials. Background Art
[0002] Due to its excellent properties such as high ion mobility, high specific surface area, and mechanics, graphene has broad application prospects in energy storage, sensing, catalysis, and composite materials. However, graphene often aggregates and accumulates due to the action of π-π bonds, which seriously reduces its comprehensive performance and hinders the further application of graphene.
[0003] Organizing graphene into a graphene aerogel with a three-dimensional network is an effective way to prevent its aggregation and accumulation, which can give full play to the excellent comprehensive properties of graphene. The unique aerogel structure also gives the material other properties, such as ultra-low density and low thermal conductivity. It is made by the sol-gel method by drying the molecular precursor (freezing or supercritical) to remove the solvent from the wet gel. Aerogels tend to show high porosity (90-99%), low density (about 3kg / m 3 ), low thermal conductivity (about 0.014 W·m at room temperature -1 ·K -1 ) and other characteristics. Therefore, they can be used in catalytic processes, electronic devices, sensors and other fields.
[0004] So far, the commonly used methods for preparing graphene aerogels are chemical reduction or hydrothermal methods, both of which require the use of complex reagents or involve complex operations. At the same time, aerogels also have the disadvantages of low strength, unstable structure, and weak elasticity. Summary of the invention
[0005] In view of the above problems, the object of the present invention is to provide a highly elastic graphene aerogel and a preparation method thereof which is simple to operate, environmentally friendly and can obtain a stable structure.
[0006] In one aspect, the present invention provides a graphene aerogel having a radially oriented structure inside.
[0007] In the present disclosure, the graphene aerogel has a radially oriented structure inside, and the existence of transverse channels effectively disperses the load and provides transverse constraints to reduce stress concentration, thereby having a more stable structure and high elastic properties.
[0008] Preferably, the graphene aerogel has a pore size distribution of 10 to 100 μm, a porosity of at least 95% (preferably at least 97%), and an apparent density of 3 to 6 mg / cm 3 .
[0009] Preferably, the plastic deformation of the graphene aerogel after 50 cycles of 50% strain is ≤15%, and the maximum stress reduction after 50 cycles of 50% strain is ≤25%. Preferably, the plastic deformation of the graphene aerogel after 50 cycles of 50% strain is ≤6%. The maximum stress value decreases slightly under 50 cycles of 50% strain. Preferably, the maximum stress reduction after 50 cycles of 50% strain is ≤15%.
[0010] On the other hand, the present invention also provides a method for preparing graphene aerogel, comprising:
[0011] (1) introducing a graphene oxide aqueous solution into a hollow copper mold until it overflows and sealing it with copper;
[0012] (2) placing a hollow copper mold filled with graphene oxide aqueous solution in a low temperature environment, first subjecting it to directional freezing and then freeze drying, to obtain graphene oxide aerogel; wherein the freezing direction of the directional freezing is from the mold surface to the liquid center;
[0013] (3) thermally reducing the obtained graphene oxide aerogel in an inert atmosphere at 800 to 1400° C. to obtain the graphene aerogel.
[0014] In the present disclosure, a structurally stable and highly elastic graphene aerogel is prepared by a special directional freezing method (centripetal freezing). On the one hand, the closed mold design makes the temperature of the contact interface between the dispersion and the mold close and lower than the center temperature of the solution in the initial state of freezing, thereby generating a temperature gradient from the surface of the solution to the center of the solution, that is, a centripetal temperature gradient, which provides a prerequisite for centripetal freezing. The growth direction of the ice crystals is parallel to the temperature gradient. Under the influence of the centripetal temperature gradient, the ice crystals grow from the inner surface of the copper mold to the center. After the solution is completely frozen, the directional growth of the ice crystals is completed. On the other hand, the graphene oxide sheets in the dispersion are squeezed to the ice crystal interface during the growth of the ice crystals, and the aerogel thus obtained forms a growth contour of centripetally oriented ice crystals. The diagonal of the longitudinal section presents a unique "bouquet-shaped" orientation. The closed cylindrical copper mold mainly produces mutually perpendicular temperature gradients on the longitudinal section. Under the action of the double gradient, the growth direction of the ice crystals converges to the diagonal. Centripetal freezing does not require complex reagents or complicated operating procedures, and can produce radial-like orientation inside the material. The existence of transverse channels effectively disperses the load and provides lateral constraints, reducing stress concentration. Based on this, it has a more stable structure and gives graphene aerogel high elastic properties.
[0015] Preferably, the concentration of the graphene oxide aqueous solution is 2-15 mg / mL, preferably 6-12 mg / mL, and more preferably 6-10 mg / mL; the diameter of the graphene oxide sheet is 5 μm-50 μm. Large-sized graphene oxide sheets have a larger bonding surface during the layer-by-layer assembly process, and the bonding is more firm.
[0016] Preferably, the freezing temperature of the directional freezing is -80°C to -196°C (liquid nitrogen environment), and the time is 2 minutes to 2 hours, preferably 2 minutes to 1 hour.
[0017] Preferably, the freeze-drying temperature is -80°C to -196°C (liquid nitrogen environment), the environment is a vacuum environment, and the vacuum degree is 1 to 100 Pa. The ice component is removed by utilizing the characteristic of direct sublimation of ice under vacuum conditions, and a lower temperature produces a higher temperature gradient, the internal structure of the aerogel has a better orientation, and a graphene oxide aerogel with a stable structure is obtained.
[0018] Preferably, the hollow mold has the following dimensions: inner diameter of 10-50 mm, height of 10-50 mm, and mold wall thickness of 1-4 mm, so as to adjust the size and internal structure of the obtained graphene aerogel sample. A thinner mold is conducive to establishing a higher temperature gradient inside. The hollow copper mold is a cubic hollow copper mold or a cylindrical hollow copper mold; preferably, the ratio of the height to the inner diameter of the hollow copper mold is 0.5-1.5.
[0019] Preferably, the inert atmosphere is an argon atmosphere; and the thermal reduction time is 1 to 4 hours.
[0020] Furthermore, preferably, the temperature of the thermal reduction is 800-1100° C. The appropriate thermal reduction temperature can better reduce the graphene oxide to reduced graphene oxide, thereby obtaining high-quality graphene aerogel.
[0021] Beneficial effects:
[0022] In the present disclosure, graphene oxide is used as a raw material, liquid nitrogen is used as a cold source, and a homemade copper mold is used to add graphene oxide to deionized water and disperse it by ultrasonic to make a uniform dispersion. Pour it into a copper mold, seal it with copper, and place it in liquid nitrogen. After it is completely frozen, take out the sample in the mold, vacuum freeze-dry it to obtain graphene oxide aerogel, and then heat-reduce it at high temperature to obtain graphene aerogel. The prepared aerogel has a stable structure and high elasticity. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The optical images of the graphene oxide aerogel and the graphene aerogel in Example 1 are shown;
[0024] Figure 2 The structural diagram of the hollow copper mold used in the present invention is shown;
[0025] Figure 3 shows a scanning electron microscope image of a longitudinal section of the graphene aerogel prepared in Example 3;
[0026] Figure 4The stress-strain curves of the graphene aerogel prepared in Example 4 under different compressive strains are shown;
[0027] Figure 5 The stress-strain curve of the graphene aerogel prepared in Example 1 after 50 compression cycles at a compression strain of 50% is shown. DETAILED DESCRIPTION
[0028] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0029] In the present disclosure, a special directional freezing method is mainly used to achieve directional growth of ice crystals, regulate the microstructure of graphene aerogel, and then improve the structural stability of the material to obtain highly elastic graphene aerogel.
[0030] In this patent, only directional freezing is used to obtain graphene aerogel with good elasticity, without complicated high-temperature transformation or the use of toxic additives, etc., which is green and efficient. The obtained aerogel has excellent performance. In this patent, the structural advantages of the mold are used to obtain graphene aerogel with good elasticity. The mechanical properties of the obtained material are relatively excellent. The following is an exemplary description of the preparation method of structurally stable and highly elastic graphene aerogel.
[0031] Dispersion of graphene oxide. Graphene oxide powder is added to deionized water and dispersed by ultrasound to obtain a uniformly dispersed graphene oxide aqueous solution (or graphene oxide dispersion). The power of the ultrasonic dispersion can be 100 to 200 W and the time can be 30 to 40 minutes.
[0032] The graphene oxide dispersion is poured into a cylindrical hollow copper mold, and the ratio of the height (h) to the diameter (inner diameter D) of the copper mold is 1:5 to 5:1, preferably 0.5 to 1. The mold is completely filled with the dispersion and sealed with copper.
[0033] Directional freezing. The sealed mold is placed in a low temperature environment for a period of time. After the dispersion in the mold is completely frozen, freeze-drying is performed to obtain graphene oxide aerogel. The directional freezing direction is from the mold surface to the liquid center, that is, the mold surface is the low temperature end, and the dispersion center is the high temperature end. The temperature of directional freezing and freeze-drying is -80°C to -196°C. The freeze-drying method is vacuum freeze-drying, which specifically includes: placing the frozen sample in a vacuum environment with a vacuum degree of 1 to 100Pa.
[0034] Thermal reduction. The graphene oxide aerogel is heated and reduced under a certain temperature and argon conditions to obtain a graphene aerogel with stable structure and high elasticity. The thermal reduction temperature is preferably 800 to 1400°C.
[0035] In the present invention, the apparent density of the obtained graphene aerogel is 3 to 7 mg / cm 3 , has excellent rebound properties. After 50 times of 50% compression strain, the rebound rate reaches more than 95%, which has important application prospects.
[0036] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0037] Example 1
[0038] (1) 320 mg of graphene oxide (thickness ~1 nm, diameter 10-50 μm) was added to 40 mL of deionized water and ultrasonically dispersed at 100 W for 30 min to obtain a uniformly dispersed graphene oxide dispersion with a concentration of 8 mg / mL;
[0039] (2) Use a self-made cylindrical copper mold with an inner diameter of φ15mm×35mm, pour the uniformly dispersed graphene oxide dispersion into the mold until it overflows, and seal the mold with a copper end cap to ensure that the inside of the mold is filled with the dispersion. Place the mold in liquid nitrogen for directional freezing (-196℃), take it out after 2 minutes, and thaw it naturally in the air for 20 minutes until the mold can be opened, and take out the sample;
[0040] (3) placing the frozen sample in a freeze dryer for vacuum drying at a vacuum degree of 1 Pa for 48 h to obtain graphene oxide aerogel;
[0041] (4) The graphene oxide aerogel was placed in a vacuum furnace, heated to 1000°C at 5°C / min in an argon atmosphere, kept at this temperature for 2 hours, and cooled naturally to obtain elastic graphene aerogel. The apparent density was about 3.6 mg / cm 3 ;
[0042] (5) The obtained aerogel was subjected to compression testing using a compression testing machine. It was found that the maximum stress value of the prepared aerogel after 50 times of 50% strain compression was slightly lower than the initial stress, and the plastic deformation was 4%.
[0043] Example 2
[0044] The only difference between Example 2 and Example 1 is that 160 mg of graphene oxide powder is added in step (1) and the concentration of the obtained dispersion is 4 mg / mL.
[0045] Example 3
[0046] The only difference between Example 3 and Example 1 is that 240 mg of graphene oxide powder is added in step (1) and the concentration of the obtained dispersion is 6 mg / mL.
[0047] Example 4
[0048] The only difference between Example 4 and Example 1 is that 400 mg of graphene oxide powder is added in step (1) and the concentration of the obtained dispersion is 10 mg / mL.
[0049] Example 5
[0050] The only difference between Example 5 and Example 1 is that 480 mg of graphene oxide powder is added in step (1) and the concentration of the obtained dispersion is 12 mg / mL.
[0051] Example 6
[0052] The only difference between Example 6 and Example 1 is that the ratio of the height (h) to the diameter (D) of the copper mold is 0.5.
[0053] Example 7
[0054] The only difference between Example 7 and Example 1 is that the ratio of the height (h) to the diameter (D) of the copper mold is 1.5.
[0055] Comparative Example 1
[0056] The only difference between Comparative Example 1 and Example 1 is that the lower surface of the hollow cylinder is -196°C and unidirectional freeze-drying is performed.
[0057] Table 1 shows the performance parameters of the graphene aerogel prepared by the present invention:
[0058]
[0059] Figure 1 Optical images of graphene oxide aerogel and graphene aerogel before and after thermal reduction are shown. After thermal reduction, the aerogel changes from yellow-brown to black graphene aerogel.
[0060] Figure 2 The structural design of the hollow copper mold is shown. The double end cap design facilitates the removal of samples after freezing, and the concave structural design leaves enough space for the volume expansion caused by water freezing, and ensures that the dispersion in the mold is in full contact with the inner surface of the mold.
[0061] Figure 3The longitudinal section scanning electron microscope image of the prepared graphene aerogel is shown. The diagonal direction presents a unique "bouquet-shaped" orientation, and the graphene sheets converge at a diagonal direction of 47°, and the convergence angle is constantly decreasing. When the longitudinal ice crystals are about to meet the transverse ice crystals at the diagonal, they will be affected by the temperature gradient caused by the transverse ice crystals. The double gradient causes the growth direction of the ice crystals to change, resulting in an "approach-compromise" trend. The closer to the center of the block, the closer the growth trend is to the common diagonal position, and the smaller the convergence angle becomes. What is special is that we can observe the following Figure 3 The special "Y"-shaped structure shown in the figure is produced when some ice crystals meet and move toward the end of growth together. The end of growth is the "Y"-shaped node. As a result, a radial orientation is generated inside the material. The existence of transverse channels effectively disperses the load and provides transverse constraints to reduce stress concentration. Based on this, it has a more stable structure and gives graphene aerogel high elastic properties.
[0062] Figure 4 The stress-strain curves of the graphene aerogel prepared in Example 4 at 10%, 20%, 30%, 40% and 50% compressive strains are shown. It can be seen from the figure that the sample exhibits good resilience under a compressive strain of 10% to 50%, and can return to its original height after the load is removed, that is, there is no obvious plastic deformation, and it exhibits good resilience.
[0063] Figure 5 The stress-strain curve of the graphene aerogel prepared in Example 1 after 50 compression cycles at a compression strain of 50% is shown. It can be seen from the figure that after the sample has undergone 50 compression cycles with a 50% strain, it still retains 96% of the maximum stress value, the sample rebound rate also reaches more than 95%, and the stress platform is only slightly reduced, indicating that it has good structural stability.
Claims
1. A graphene aerogel, characterized in that: The graphene aerogel has a radial orientation structure inside; The graphene aerogel has a plastic deformation of ≤15% after 50 cycles of 50% strain, and a maximum stress reduction of ≤25% after 50 cycles of 50% strain; The preparation method of the graphene aerogel comprises: (1) introducing a graphene oxide aqueous solution into a hollow copper mold until it overflows and sealing it with copper; the concentration of the graphene oxide aqueous solution is 2 to 15 mg / mL; (2) placing a hollow copper mold filled with graphene oxide aqueous solution in a low temperature environment, first subjecting it to directional freezing and then freeze drying, to obtain graphene oxide aerogel; the freezing direction of the directional freezing is from the mold surface to the center of the liquid; (3) thermally reducing the obtained graphene oxide aerogel in an inert atmosphere at 800 to 1400° C. to obtain the graphene aerogel; Among them, there is a "Y"-shaped channel structure between the graphene sheets inside the graphene aerogel, which is formed by the convergence of transverse ice crystals and longitudinal ice crystals at the diagonal of the mold.
2. The graphene aerogel according to claim 1, characterized in that: The graphene aerogel has a pore size distribution of 10 to 100 μm, a porosity of at least 95%, and an apparent density of 3 to 6 mg / cm 3 .
3. The graphene aerogel according to claim 1, characterized in that: The sheet diameter of the graphene oxide is 5 μm to 50 μm.
4. The graphene aerogel according to claim 1, characterized in that: The concentration of the graphene oxide aqueous solution is 6-12 mg / mL.
5. The graphene aerogel according to claim 1, characterized in that: The freezing temperature of the directional freezing is -80°C to -196°C, and the time is 2 minutes to 2 hours.
6. The graphene aerogel according to claim 1, characterized in that: The freeze-drying temperature is -80°C to -196°C, the environment is a vacuum environment, and the vacuum degree is 1Pa to 100Pa.
7. The graphene aerogel according to claim 1, characterized in that: The dimensions of the hollow copper mold are: an inner diameter of 10 to 50 mm, a height of 10 to 50 mm, and a mold wall thickness of 1 to 4 mm; the hollow copper mold is a cubic hollow copper mold or a cylindrical hollow copper mold.
8. The graphene aerogel according to claim 7, characterized in that: The ratio of the height to the inner diameter of the cylindrical hollow copper mold is 0.5 to 1.
5.
9. The graphene aerogel according to claim 1, characterized in that: The temperature of the thermal reduction is 800-1100°C.
10. The graphene aerogel according to claim 1, characterized in that: The inert atmosphere is an argon atmosphere; the thermal reduction time is 1 to 4 hours.