Preparation method of battery grade manganese sulfate

By adjusting the pH of copper manganese liquid and using soluble sulfides and saponified bis(2,4,4-trimethylpentyl)phosphinic acid extractant, the problems of complicated processes and large manganese losses in the prior art are solved. It realizes efficient and low-cost battery-grade manganese sulfate preparation, simplifies the process and improves the purity and conversion rate of the product.

CN115893498BActive Publication Date: 2024-11-15GUANGDONG JIANA ENERGY TECH CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211464189.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-15
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

The existing battery-grade manganese sulfate preparation methods are complicated, and the extraction agent P204 is difficult to effectively separate calcium and manganese under specific pH conditions, resulting in large loss of manganese and high drainage treatment costs and high solubility.

Method used

By adjusting the pH of the copper-manganese liquid to 2.0-3.0, heavy metals such as copper and zinc were precipitated with soluble sulfides, and then manganese was extracted with saponified bis(2,4,4-trimethylpentyl)phosphinic acid extractant. , combined with sulfuric acid pickling, achieve efficient separation of manganese and calcium, reduce the introduction of impurities, and improve the conversion rate of manganese.

Benefits of technology

It realizes efficient and low-cost preparation of battery-grade manganese sulfate, reducing the loss of manganese and drainage treatment costs, simplifying the process, and improving the conversion rate and product purity of manganese.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115893498B_ABST
    Figure CN115893498B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of manganese sulfate preparation process, and in particular to a method for preparing battery-grade manganese sulfate. The method for preparing battery-grade manganese sulfate of the present application includes: collecting copper-manganese solution; adjusting the pH of the copper-manganese solution to 2.0-3.0, and then precipitating the copper-manganese solution with a soluble sulfide, and separating the solid and liquid to obtain a filtrate with a pH of 4.0-5.0; extracting manganese from the filtrate with a saponified di(2,4,4-trimethylpentyl)phosphine acid extractant to obtain a loaded organic phase and a raffinate; cleaning the calcium, magnesium, and sodium in the loaded organic phase, and then washing with sulfuric acid to obtain battery-grade manganese sulfate. The preparation method of the present application has a high conversion rate of manganese in copper-manganese solution, introduces few impurities, and can be used in industry to prepare battery-grade manganese sulfate at low cost and high efficiency, with good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of manganese sulfate preparation technology, and in particular relates to a method for preparing battery-grade manganese sulfate. Background Art

[0002] Manganese sulfate is a typical representative of manganese compounds. It can be used to produce metallic manganese, other manganese salts and manganese oxides. It is widely used in energy, medicine, fertilizer, feed, food, papermaking, catalyst and other industries. Among them, battery-grade manganese sulfate is used as a raw material for the preparation of battery materials such as nickel-cobalt-manganese ternary precursors and lithium manganese iron phosphate. Its future demand will grow rapidly. There are generally two process routes for battery-grade manganese sulfate. The first is to electrolyze manganese metal sheets and add sulfuric acid for acid dissolution to obtain manganese sulfate. The second is to start from the ore and obtain high-purity manganese sulfate through reduction, impurity removal and crystallization. The use of copper-manganese liquid produced in the extraction process of cobalt hydrometallurgy to prepare manganese metal salts can realize the resource utilization of manganese in cobalt intermediates, which not only reduces the waste of resources, but also increases economic benefits. It has been widely studied.

[0003] At present, the preparation of manganese metal salts using copper-manganese solution mainly includes three processes: removing heavy metals such as copper and zinc, removing calcium, and preparing manganese metal salts. Patent document CN110172581A discloses a method for preparing battery-grade manganese sulfate from reverse copper-manganese solution, which sequentially removes copper from the reverse copper-manganese solution of the sulfuric acid system by electrolytic manganese powder replacement, extracts deep copper removal, extracts zinc and calcium with extractant P204, removes impurities deeply with hydrogen sulfide gas, adjusts pH with electrolytic manganese powder, and evaporates, concentrates, and crystallizes the solution to obtain a battery-grade manganese sulfate product. This method has many processing steps and is cumbersome, and the extractant P204 has difficulty in separating calcium and manganese when the solution pH is 1.8 to 2.2, which will cause a large loss of manganese. Patent document CN108585051B discloses a method for preparing battery-grade manganese sulfate from copper-manganese chloride solution, which sequentially neutralizes copper ions in the solution with manganese carbonate, precipitates heavy metal ions with manganese sulfide, preliminarily precipitates calcium ions with manganese sulfate, and deeply precipitates calcium ions with active manganese fluoride, and then adds concentrated sulfuric acid to react and synthesize crude manganese sulfate crystals, which are then recrystallized to obtain battery-grade manganese sulfate crystals. This method deeply precipitates calcium ions with active manganese fluoride, and fluoride ions are present in the solution, which greatly increases the treatment cost of wastewater in the later stage of production. In addition, the solubility of manganese sulfate is relatively large, and it is difficult to produce manganese sulfate crystals by adding concentrated sulfuric acid. Summary of the invention

[0004] The purpose of the present application is to provide a method for preparing battery-grade manganese sulfate, aiming to solve the problem of how to efficiently prepare battery-grade manganese sulfate from copper-manganese solution.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] The present application provides a method for preparing battery-grade manganese sulfate, comprising:

[0007] Collect copper-manganese solution;

[0008] The pH of the copper-manganese solution is adjusted to 2.0-3.0, and then the copper-manganese solution is precipitated with a soluble sulfide, and a filtrate with a pH of 4.0-5.0 is obtained by solid-liquid separation;

[0009] The filtrate is subjected to manganese extraction treatment using a saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to obtain a loaded organic phase and a raffinate;

[0010] The calcium, magnesium and sodium in the loaded organic phase are cleaned and then pickled with sulfuric acid to obtain battery-grade manganese sulfate.

[0011] In one embodiment, the precipitation treatment of the copper-manganese solution with the soluble sulfide includes: heating the copper-manganese solution with a pH of 2.0 to 3.0 to 45° C. to 55° C., and then adding the soluble sulfide to carry out stirring reaction.

[0012] In one embodiment, the soluble sulfide is selected from at least one of sodium sulfide and ammonium sulfide; and / or,

[0013] The amount of soluble sulfide used is 1 to 2 times the total molar amount of copper and zinc in the copper-manganese solution.

[0014] In one embodiment, the total volume of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant is 100%, and the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant includes: 15% to 25% of saponified di(2,4,4-trimethylpentyl)phosphinic acid and 75% to 85% of sulfonated kerosene.

[0015] In one embodiment, the saponification rate of the saponified di(2,4,4-trimethylpentyl)phosphinic acid is 40% to 45%.

[0016] In one embodiment, the volume ratio of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to the filtrate is 13-14:1.

[0017] In one embodiment, the manganese extraction process is a four-stage countercurrent extraction process, and the temperature during the manganese extraction process is 45°C to 55°C.

[0018] In one embodiment, washing the calcium, magnesium and sodium in the loaded organic phase comprises: counter-current washing the loaded organic phase with a first sulfuric acid solution having a pH of 2.5 to 3.5;

[0019] Alternatively, the loaded organic phase is countercurrently washed with a hydrochloric acid solution having an acidity of 0.1 to 0.3 N, and then countercurrently washed with water.

[0020] In one embodiment, the sulfuric acid pickling to obtain battery-grade manganese sulfate includes: pickling with a second sulfuric acid solution with an acidity of 4-6N, and the volume ratio of the loaded organic phase to the second sulfuric acid solution is 9-11:1.

[0021] In one embodiment, the preparation method further comprises: adding anhydrous calcium sulfate seeds and soluble sulfate to the raffinate for decalcification to obtain a recoverable decalcified filtrate having a calcium content of ≤1 g / L.

[0022] The preparation method of battery-grade manganese sulfate provided by the present application uses copper-manganese liquid as a raw material, and uses soluble sulfides to precipitate and remove most of the heavy metals such as copper and zinc in the copper-manganese liquid under the condition that the pH of the copper-manganese liquid is 2.0 to 3.0, and the process does not introduce other difficult-to-remove impurities. The filtrate obtained after precipitation and separation is treated with saponified di(2,4,4-trimethylpentyl)phosphine acid extractant under the condition of pH 4.0 to 5.0 for manganese extraction. Under this condition, the calcium ion concentration in the filtrate is not easy to affect the manganese extraction effect, so that manganese and calcium can be well separated, and most of the calcium is left in the raffinate, thereby obtaining a highly manganese-loaded organic phase, and the calcium, magnesium, and sodium in the loaded organic phase are further cleaned later, and finally sulfuric acid pickling can obtain battery-grade manganese sulfate. The preparation method has a high conversion rate for manganese in copper-manganese liquid, introduces few impurities, and can be used in industry to prepare battery-grade manganese sulfate at low cost and high efficiency, and has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 This is a schematic flow chart of a method for preparing battery-grade manganese sulfate provided in an embodiment of the present application;

[0025] Figure 2 is a graph showing the relationship between the extraction of metal ions by the extractant Kzu272 provided in the examples of the present application and the equilibrium pH;

[0026] Figure 3 This is the specific process flow of the method for preparing battery-grade manganese sulfate provided in the examples of the present application. DETAILED DESCRIPTION

[0027] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0028] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0029] In the present application, "at least one" means one or more, "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items.

[0030] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0031] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0032] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0033] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0034] The first aspect of the present application provides a method for preparing battery-grade manganese sulfate, such as Figure 1 As shown, the following steps are included:

[0035] S01: Collect copper-manganese solution;

[0036] S02: adjusting the pH of the copper-manganese solution to 2.0-3.0, then precipitating the copper-manganese solution with a soluble sulfide, and performing solid-liquid separation to obtain a filtrate with a pH of 4.0-5.0;

[0037] S03: extracting manganese from the filtrate using a saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to obtain a loaded organic phase and a raffinate;

[0038] S04: The calcium, magnesium and sodium in the loaded organic phase are cleaned and then washed with sulfuric acid to obtain battery-grade manganese sulfate.

[0039] The preparation method of battery-grade manganese sulfate provided in the present application uses copper-manganese liquid as raw material, and sequentially undergoes three general processes of sulfide precipitation, manganese extraction treatment, and sulfuric acid pickling of the loaded organic phase, thereby obtaining the final battery-grade sulfuric acid product. Specifically, most of the heavy metals such as copper and zinc in the copper-manganese liquid are precipitated and removed with soluble sulfides under the condition that the pH of the copper-manganese liquid is 2.0-3.0, and the process does not introduce other difficult-to-remove impurities, and then the filtrate obtained after the precipitation separation is treated with saponified di(2,4,4-trimethylpentyl)phosphine acid extractant under the condition of pH 4.0-5.0. Under this condition, the calcium ion concentration in the filtrate is not easy to affect the manganese extraction effect, so that manganese and calcium can be well separated, and most of the calcium remains in the raffinate, thereby obtaining a highly manganese loaded organic phase, and the calcium, magnesium, and sodium in the loaded organic phase are further cleaned later, and finally sulfuric acid pickling can obtain battery-grade manganese sulfate. This preparation method has a high conversion rate of manganese in copper-manganese liquid, introduces few impurities, and can be used to prepare battery-grade manganese sulfate in industry at low cost and high efficiency, with good application prospects.

[0040] In the above step S01, the collected copper-manganese solution can be a copper-manganese chloride solution produced in the extraction process of cobalt hydrometallurgy. Generally, the copper-manganese chloride solution produced by cobalt hydrometallurgy often contains Mn, Cu, Zn, Ca, and metal ions such as Mg and Co with lower content. For example, the content of each element in the copper-manganese chloride solution can be: Mn 70-110g / L, Cu 1-10g / L, Zn 5-15g / L, Ca 8-15g / L, Mg 0.01-0.1g / L, Co 0.01-0.2g / L. The pH of the copper-manganese solution produced by cobalt hydrometallurgy is generally between 1.0 and 1.5.

[0041] The above step S02 is a process of removing the weight of soluble sulfides.

[0042] Specifically, the pH of the collected copper-manganese solution is first adjusted to 2.0-3.0, and then the copper-manganese solution is precipitated with a soluble sulfide. A soluble carbonate can be added to the copper-manganese solution to adjust the acidity so that the pH of the copper-manganese solution is 2.0-3.0. The soluble calcium carbonate can be ammonium carbonate or sodium carbonate (i.e., soda ash). Under the condition of pH=2.0-3.0, heavy metals such as Cu, Zn, and Co in the copper-manganese solution can be well precipitated by sulfides.

[0043] In one embodiment, the precipitation treatment of the copper-manganese solution with the soluble sulfide includes: heating the copper-manganese solution with a pH of 2.0 to 3.0 to 45° C. to 55° C., and then adding the soluble sulfide to carry out stirring reaction. The copper-manganese solution at a temperature of 45° C. to 55° C. can make the soluble sulfide dissolve better and fully carry out the precipitation reaction.

[0044] In one embodiment, the soluble sulfide is selected from at least one of sodium sulfide and ammonium sulfide; the above-mentioned soluble sulfide can not only precipitate heavy metals such as Cu and Zn well, but also does not introduce iron impurities that are difficult to remove, so it is not easy to affect the purity of subsequent battery-grade manganese sulfate. The amount of soluble sulfide is 1 to 2 times the total molar amount of copper and zinc in the copper-manganese solution, so that most of the copper and zinc in the copper-manganese solution are precipitated, and the Cu and Zn content in the final filtrate is substantially less than 0.0010 g / L.

[0045] The pH value of the filtrate can be adjusted to 4.0-5.0 by first performing solid-liquid separation after the precipitation treatment, and then adding soluble carbonate to the filtrate obtained by solid-liquid separation to adjust the pH of the filtrate to 4.0-5.0. Alternatively, after the precipitation treatment, directly adding soluble carbonate to adjust the pH of the liquid to 4.0-5.0, and then performing solid-liquid separation to obtain a filtrate with a pH of 4.0-5.0; wherein the soluble carbonate for acid adjustment can be ammonium carbonate or sodium carbonate.

[0046] The above step S03 is a process of extracting manganese. Specifically, before extracting manganese, the filtrate with a pH of 4.0 to 5.0 obtained above can be used as an extraction liquid. After obtaining the filtrate with a pH of 4.0 to 5.0, the filtrate is treated with a saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to extract manganese to obtain a loaded organic phase and a raffinate. Under this condition, the concentration of calcium ions has little effect on the manganese extraction effect, so there is no need to use fluoride for deep decalcification, and the extraction to achieve anion exchange is highly industrially operable.

[0047] The structure of di(2,4,4-trimethylpentyl)phosphinic acid is as follows:

[0048]

[0049] The di(2,4,4-trimethylpentyl)phosphinic acid used as the extractant is referred to as Kzu272. The relationship between the extraction of metal ions by Kzu272 and the equilibrium pH is as follows Figure 2 As shown. It can be seen that when the pH of the feed liquid is 4.0-4.5, the extraction rate of copper and zinc by Kzu272 is about 100%, and the curves of copper extraction and manganese extraction are similar, which makes separation extremely difficult. Therefore, the present application first uses chemical sulfide precipitation to precipitate copper and zinc to reduce the steps and reagent consumption of manganese extraction and separation. The extraction process at a pH of 4.0-4.5 can basically separate calcium and manganese. If the pH value is further lowered to control the Kzu272 extractant to not extract calcium at all, the residual manganese content in the raffinate will be high. If the pH value is further increased to control the Kzu272 extractant to extract all manganese, more than 80% of the calcium in the feed liquid will also be extracted. In this way, the subsequent washing and separation will cause a large loss of manganese. Therefore, it is comprehensively considered to extract manganese at a pH of 4.0-4.5, and then add a calcium cleaning treatment step (which can remove calcium, magnesium, and sodium). In this way, the purpose of efficiently recovering manganese to prepare battery-grade manganese sulfate can be achieved through the previous step of sulfidation precipitation of copper and zinc, extraction of manganese at pH = 4.0-4.5 and subsequent cleaning treatment.

[0050] In one embodiment, the total volume of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant is 100%, and the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant includes: 15% to 25% of saponified di(2,4,4-trimethylpentyl)phosphinic acid and 75% to 85% of sulfonated kerosene. This has a better extraction effect on manganese. Furthermore, the saponification rate of the saponified di(2,4,4-trimethylpentyl)phosphinic acid is 40% to 45%, and specifically, 10 mol / L NaOH solution can be used as a saponifying agent for saponification.

[0051] In one embodiment, the volume ratio of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to the filtrate is 13 to 14:1. Further, the manganese extraction treatment is a four-stage countercurrent extraction treatment, and the temperature in the manganese extraction treatment is 45°C to 50°C. Among them, in the four-stage countercurrent extraction treatment, the extraction time can be 4 to 6 minutes, the stirring speed is 250 to 350 r / min, and the standing time is 8 to 12 minutes. The experimental temperature is 45 to 50°C, and the pH value of the raffinate is controlled to remain unchanged to obtain a loaded organic phase and a raffinate.

[0052] The loaded organic phase is used to recover manganese. The raffinate is rich in calcium and can be recycled after decalcification. In one embodiment, anhydrous calcium sulfate seeds and soluble sulfate are added to the raffinate for decalcification to obtain a recyclable decalcified filtrate with a calcium content of ≤1g / L. The raffinate is rich in calcium, and the decalcified filtrate obtained after decalcification of the raffinate can be added with hydrochloric acid to adjust the acid and returned to the front end for the anti-copper-manganese process of cobalt wet extraction, or the decalcified filtrate obtained by decalcification of the raffinate can be used as an acid wash in the extraction process after acid adjustment.

[0053] Specifically, the raffinate is heated to 85-90° C., anhydrous calcium sulfate seeds and soluble sulfate are added to the raffinate at 10 g / L (the amount of soluble sulfate added is 1.5 times the amount of calcium), stirred for 1-2 hours, and the Ca content solution is detected after the reaction is complete. When the Ca content is ≤1 g / L, the calcium-removing filtrate is filtered to obtain the calcium-removing filtrate. The soluble sulfate can be one or more of sodium sulfate, manganese sulfate, and ammonium sulfate.

[0054] The above step S04 is a step for forming the final target product, battery-grade manganese sulfate. Specifically, calcium, magnesium and sodium in the loaded organic phase obtained after manganese extraction are first washed, and then washed with sulfuric acid to obtain battery-grade manganese sulfate.

[0055] Among them, the step of cleaning the calcium, magnesium and sodium in the loaded organic phase can be cleaned in two ways according to the amount of calcium. Specifically, on the one hand, if the calcium content in the loaded organic phase obtained after manganese extraction is relatively small, the cleaning step may include: countercurrent washing the loaded organic phase with a first sulfuric acid solution with a pH of 2.5 to 3.5; the sulfuric acid solution under this condition can wash a small amount of calcium and magnesium and sodium in the loaded organic phase. On the other hand, if the calcium content in the loaded organic phase obtained after manganese extraction is relatively high, the loaded organic phase can be countercurrently washed with a hydrochloric acid solution with an acidity of 0.1 to 0.3N, and then countercurrently washed with water, so that not only the calcium can be washed with magnesium and sodium, but also the chloride ions mixed in the loaded organic phase can be removed.

[0056] In one embodiment, the final sulfuric acid pickling to obtain battery-grade manganese sulfate includes: pickling with a second sulfuric acid solution with an acidity of 4 to 6N, and the volume ratio of the loaded organic phase to the second sulfuric acid solution is 9 to 11: 1. Under this condition, most of the manganese in the loaded organic phase can be obtained, thereby obtaining battery-grade manganese sulfate. Further, the sulfuric acid pickling can be a five-stage countercurrent washing.

[0057] In one embodiment, if Figure 3 As shown, the preparation method of battery-grade manganese sulfate includes:

[0058] Step 1, weight removal of soluble sulfides: Add carbonate to the copper-manganese solution to adjust the acidity and adjust the pH to 2.0-3.0. Heat to 45-55°C, add sulfide to react for 2-3 hours, and filter to obtain filter residue (can be sold) and filtrate after the reaction is complete. The filtrate is tested for Cu and Zn contents less than 0.0010 g / L, and the pH is adjusted to 4.0-4.5 with carbonate and filtered. The filtrate is used as the extraction liquid.

[0059] Step 2, Kzu272 manganese extraction: The extractant Kzu272 after saponification (Kzu272 accounts for 15-25% by volume, sulfonated kerosene diluent accounts for 75-85 by volume; Kzu272 saponification rate is 40%-45%, and the saponifier is 10 mol / L NaOH solution) is used to perform four-stage countercurrent extraction on the extractant solution of step 1, and the ratio of the extractant to the extractant solution is 13-14:1. When the pH value of the raffinate is controlled to be unchanged, the loaded organic phase and the raffinate are obtained. A small amount of calcium, magnesium and sodium ions in the loaded organic phase are washed, and finally a 4-6N sulfuric acid solution is used to perform five-stage countercurrent washing on the loaded organic phase to obtain a battery-grade manganese sulfate solution.

[0060] Step 3, decalcification of the raffinate: The raffinate of step 2 is heated to 85-90°C, and anhydrous calcium sulfate seeds and soluble sulfate such as sodium sulfate are added to the raffinate at a rate of 10 g / L (the amount of sodium sulfate added = the amount of calcium * 1.5), and the mixture is stirred for reaction for 2 hours. After the reaction is complete, the Ca content solution is tested, and when the Ca content is ≤1 g / L, the decalcified filtrate is filtered to obtain the decalcified filtrate. The decalcified filtrate is acidified with hydrochloric acid and can be returned to the front end for the reverse copper and manganese process of cobalt wet extraction.

[0061] In summary, the preparation method of the battery-grade manganese sulfate has fewer steps, and uses sulfide to remove heavy metals such as Cu and Zn, without introducing difficult-to-remove iron impurities. When the Kzu272 extraction is carried out at a solution pH of 4.0 to 4.5, the concentration of calcium ions has almost no effect on the manganese extraction effect, and there is no need to use fluoride for deep calcium removal. In addition, the extraction to achieve anion exchange has strong industrial operability. The loaded organic phase after extraction is easily washed to obtain battery-grade manganese sulfate. The raffinate is decalcified by a soluble sulfate, and after acid adjustment with hydrochloric acid, it can be returned to the front end for the reverse copper-manganese process of cobalt wet extraction. The conversion rate of manganese in the entire process of preparing battery-grade manganese sulfate from copper-manganese liquid is high, and the battery-grade purity requirement can be met.

[0062] The following describes the invention in conjunction with specific embodiments.

[0063] Example 1

[0064] A method for preparing battery-grade manganese sulfate comprises the following steps:

[0065] Step 1: Soluble sulfide weight removal:

[0066] Provide copper manganese chloride solution, detect the pH, Mn, Zn, Co, Cu, Ca, Mg and other ions of the copper manganese chloride solution, take 3L of copper manganese solution in a 5L beaker, add 7g of soda ash to adjust the acid, and adjust the pH to 2.15. Heat to 50°C, add 13.7g of sodium sulfide to react for 2h. Use soda ash to adjust the acid, adjust the pH to 4.5, filter, and use the filtrate as the extraction liquid. The composition of the copper manganese chloride solution and the extraction liquid is shown in Table 1.

[0067] Table 1

[0068]

[0069] Step 2: Extraction of manganese with extractant Kzu272:

[0070] The extractant in step 1 was subjected to a four-stage countercurrent extraction using saponified Kzu272 (volume fraction 20%, diluent sulfonated kerosene, saponification rate 40%, saponifier 10 mol / L NaOH solution), the ratio of extractant to extractant was 13:1, the extraction time was 5 min, the stirring speed was 300 r / min, the standing time was 10 min, the experimental temperature was 50 ° C, and the pH value of the raffinate was controlled to be unchanged to obtain the loaded organic phase and the raffinate. The pH value of H was 3. 2 SO 4 The loaded organic phase was subjected to a second-stage countercurrent wash to remove a small amount of calcium, magnesium and sodium ions in the loaded organic phase. 2 SO 4 The loaded organic phase was subjected to 5-stage countercurrent washing, and the ratio of the loaded organic phase to sulfuric acid was 10:1, to obtain a battery-grade manganese sulfate solution. The components of the extract, the battery-grade manganese sulfate solution, and the raffinate are shown in Table 2.

[0071] Table 2

[0072]

[0073] Step 3: Decalcification of the raffinate:

[0074] Take 3L of raffinate in a 5L beaker, heat it to 90°C, add 30g of anhydrous calcium sulfate seeds to the raffinate, and add 160.12g of sodium sulfate, stir and react for 2h and filter. The filtrate is acidified with hydrochloric acid to 4.5N and then returned to the front end for the reverse copper and manganese process of cobalt wet extraction. The composition of the filtrate is shown in Table 3.

[0075] Table 3

[0076]

[0077] Example 2

[0078] A method for preparing battery-grade manganese sulfate comprises the following steps:

[0079] Step 1, weight removal of soluble sulfide: same as in Example 1.

[0080] Step 2: Extraction of manganese with extractant Kzu272:

[0081] The extractant in step 1 of Example 1 was subjected to a four-stage countercurrent extraction using saponified Kzu272 (volume fraction of 20%, diluent of sulfonated kerosene, saponification rate of 40%, saponifier of 10 mol / L NaOH solution), the ratio of extractant to extractant was 14:1, the extraction time was 5 min, the stirring speed was 300 r / min, the extraction was allowed to stand for 10 min, the experimental temperature was 50 ° C, and the pH value of the raffinate was controlled to be constant to obtain the loaded organic phase and the raffinate. The loaded organic phase was subjected to a two-stage countercurrent washing using 0.2N HCl to remove calcium, magnesium and sodium ions in the loaded organic phase. The loaded organic phase was then subjected to a three-stage countercurrent washing using pure water to remove chloride ions mixed in the loaded organic phase, and finally 5N H 2 SO 4 The loaded organic phase was subjected to 5-stage countercurrent washing, and the ratio of the loaded organic phase to sulfuric acid was 10:1, to obtain a battery-grade manganese sulfate solution. The components of the extract, the battery-grade manganese sulfate solution, and the raffinate are shown in Table 4.

[0082] Table 4

[0083]

[0084] Example 3

[0085] A method for preparing battery-grade manganese sulfate comprises the following steps:

[0086] Step 1, weight removal of soluble sulfide: same as in Example 1.

[0087] Step 2: Extraction of manganese with extractant Kzu272:

[0088] The extractant in step 1 of Example 1 was subjected to a four-stage countercurrent extraction using saponified Kzu272 (volume fraction of 20%, diluent of sulfonated kerosene, saponification rate of 50%, saponifier of 10 mol / L NaOH solution), the ratio of extractant to extractant was 13:1, the extraction time was 5 min, the stirring speed was 300 r / min, the extraction was allowed to stand for 10 min, the experimental temperature was 50 ° C, and the pH value of the raffinate was controlled to be constant to obtain the loaded organic phase and the raffinate. The loaded organic phase was subjected to a two-stage countercurrent washing using 0.2N HCl to remove calcium, magnesium and sodium ions in the loaded organic phase. The loaded organic phase was then subjected to a three-stage countercurrent washing using pure water to remove chloride ions mixed in the loaded organic phase, and finally 5N H 2 SO 4 The loaded organic phase was subjected to 5-stage countercurrent washing, and the ratio of the loaded organic phase to sulfuric acid was 10:1, to obtain a battery-grade manganese sulfate solution. The composition of the extract, the battery-grade manganese sulfate solution, and the raffinate are shown in Table 5.

[0089] Table 5

[0090]

[0091] Comparative Example 1

[0092] A method for preparing battery-grade manganese sulfate comprises the following steps:

[0093] The copper manganese chloride solution (see Table 1) is collected, and then the copper manganese chloride solution is sequentially neutralized with manganese carbonate to precipitate copper ions, manganese sulfide to precipitate heavy metal ions, manganese sulfate to preliminarily precipitate calcium ions, and active manganese fluoride to deeply precipitate calcium ions, and then reacted with concentrated sulfuric acid to synthesize crude manganese sulfate crystals; the crude manganese sulfate crystals are recrystallized to obtain battery-grade manganese sulfate crystals.

[0094] Referring to patent CN108585051B, a saturated manganese sulfate solution is added dropwise to the copper chloride manganese liquid after heavy metal removal according to the molar ratio of calcium ions to manganese sulfate of 1.0: (2.0-4.0), and after the addition is completed, the reaction is continued at 25-30°C for 1.5-2.0 hours under stirring conditions, and after the reaction is completed, the calcium sulfate precipitate residue and the preliminary decalcified liquid are obtained by vacuum filtration. Manganese fluoride powder is added according to the molar ratio of the remaining calcium ions and manganese fluoride in the preliminary decalcified liquid of 1.0: (2.5-3.5), and the temperature is raised to 70-80°C and stirred for 2.0-2.5 hours. After the reaction is completed, it is allowed to stand for aging for 5.0-6.0 hours, and the calcium fluoride precipitate residue and the deep decalcified liquid are obtained by vacuum filtration. The liquid after deep decalcification is placed in an anti-corrosion reactor, and concentrated sulfuric acid is added dropwise under continuous stirring at a molar ratio of manganese ions to sulfuric acid of 1.0: (0.95-1.05). After the addition is completed, the reaction is continued at 90-95°C for 1.0-2.5 hours. After the reaction is completed, centrifugation is performed while hot to obtain crude manganese sulfate crystals. The primary manganese sulfate mother liquor is returned to the crude manganese sulfate crystal synthesis process, and the primary manganese sulfate crystals are added to the tertiary crystal mother liquor for secondary recrystallization to obtain the secondary crystal mother liquor and the secondary manganese sulfate crystals; the secondary manganese sulfate crystals are added to the quaternary crystal mother liquor for tertiary recrystallization to obtain the tertiary crystal mother liquor and the tertiary manganese sulfate crystals; and so on, 5-stage countercurrent recrystallization is performed, and battery-grade manganese sulfate is obtained after centrifugation.

[0095] In this comparative example, calcium ions are deeply precipitated by active manganese fluoride, and fluoride ions exist in the solution, which greatly increases the treatment cost of wastewater in the later stage of production. In addition, manganese sulfate has a large solubility, and it is difficult to produce manganese sulfate crystals by adding concentrated sulfuric acid in industry.

[0096] Comparative Example 2

[0097] A method for preparing battery-grade manganese sulfate comprises the following steps:

[0098] Collect the copper manganese chloride solution, see Table 1.

[0099] Referring to patent CN110172581 A, the copper manganese chloride solution was allowed to stand for 4 hours to separate into layers, and the residual organic solvent in the upper layer was removed. An appropriate amount of electrolytic manganese powder ≥ 325 mesh was added to the reverse copper manganese solution, and stirred for 2 hours. The final pH value was controlled to be 2.0-2.5, and the copper was extracted by countercurrent fractional extraction process after filtration, and the raffinate contained Cu < 0.5 g / L. Continue to use electrolytic manganese powder ≥325 mesh to adjust the pH value of the extract to 1.8-2.2, react for 3 hours, control the solution to contain 30-45g / L of Mn after concentration, filter and use multi-stage cross-current extraction to control the P204 concentration to 0.7-1.5mol / L, extraction temperature to 40-55℃, ratio (4:1)-(8:1), contact time to 2.5-4min, stage number 4-8, control the raffinate Cu <0.001g / L, Fe <0.001g / L, Ca <0.01g / L, Zn <0.001g / L. Add 0.0012mol H 2 S gas is introduced into the above raffinate, the reaction temperature is controlled at 50°C, the reaction time is 3.5 hours, and after filtration, the pH value is adjusted to 4.5 using electrolytic manganese powder ≥325 mesh, the reaction time is 3.5 hours, the solution is evaporated, concentrated and crystallized, and centrifuged while hot to obtain manganese sulfate solid, which is then dried at a low temperature of ≤105°C to obtain a battery-grade manganese sulfate product.

[0100] The preparation steps of this comparative example are many and complicated, and when the pH value of the solution of P204 extractant is 1.8-2.2, it is difficult to separate Ca and Mn, which will cause a large loss of manganese.

[0101] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing battery-grade manganese sulfate, characterized in that: include: Collect copper-manganese solution; The copper-manganese solution comprises: Mn 70-110 g / L, Cu 1-10 g / L, Zn 5-15 g / L, Ca 8-15 g / L, Mg 0.01-0.1 g / L, Co 0.01-0.2 g / L; The pH of the copper-manganese solution is adjusted to 2.0-2.15, and then the copper-manganese solution is precipitated with a soluble sulfide to obtain a filtrate with a pH of 4.37-5.0 by solid-liquid separation; The filtrate is subjected to manganese extraction treatment with a saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to obtain a loaded organic phase and a raffinate; the saponification rate of the saponified di(2,4,4-trimethylpentyl)phosphinic acid is 50%, and the volume ratio of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant to the filtrate is 13:1; the total volume of the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant is 100%, and the saponified di(2,4,4-trimethylpentyl)phosphinic acid extractant comprises: 20% of saponified di(2,4,4-trimethylpentyl)phosphinic acid and 80% of sulfonated kerosene; The calcium, magnesium and sodium in the loaded organic phase are cleaned and then pickled with sulfuric acid to obtain battery-grade manganese sulfate; Wherein, washing the calcium, magnesium and sodium in the loaded organic phase comprises: counter-currently washing the loaded organic phase with a hydrochloric acid solution having an acidity of 0.2N, and then counter-currently washing with water; The sulfuric acid pickling to obtain battery-grade manganese sulfate includes: pickling with a sulfuric acid solution with an acidity of 5N, and the volume ratio of the loaded organic phase to the sulfuric acid solution is 10:

1.

2. The preparation method according to claim 1, characterized in that The precipitation treatment of the copper-manganese solution with soluble sulfide includes: heating the copper-manganese solution with pH=2.0-2.15 to 45° C.-55° C., and then adding the soluble sulfide to carry out stirring reaction.

3. The preparation method according to claim 2, characterized in that: The soluble sulfide is selected from at least one of sodium sulfide and ammonium sulfide; and / or, The amount of the soluble sulfide used is 1 to 2 times the total molar amount of copper and zinc in the copper-manganese solution.

4. The preparation method according to claim 1, characterized in that: The manganese extraction process is a four-stage countercurrent extraction process, and the temperature in the manganese extraction process is 45°C to 55°C.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The preparation method further comprises: adding anhydrous calcium sulfate seeds and soluble sulfate to the raffinate for decalcification to obtain a recyclable decalcified filtrate with a calcium content of ≤1 g / L.

Citation Information

Patent Citations

  • A method for preparing battery-grade manganese sulfate from copper chloride manganese solution

    CN108585051B

  • Method for preparing battery-grade manganese sulfate from reverse copper-manganese liquid

    CN110172581A

  • Method for preparing high-purity manganese sulfate from manganese-containing waste liquid

    CN104445424A

  • Method for preparing battery-grade manganese sulfate

    CN112079391A

  • Method for preparing nickel / manganese / lithium / cobalt sulfate and tricobalt tetraoxide from battery wastes

    US20190152797A1