A rare earth iron alloy cored wire and preparation method thereof
By using rare earth iron alloy cored wire in steel smelting, the problems of low rare earth yield and uneven distribution are solved. By increasing the melting point and density, preventing oxidation and floating, more efficient rare earth utilization and steel quality improvement are achieved.
Patent Information
- Application Number
- CN202211418378.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-14
AI Technical Summary
In the steel smelting process, the yield of rare earths is low and the distribution is uneven. Pure rare earths have a low melting point and low density, which makes them easy to float and affect the physical and chemical properties of the mold slag. They are also easy to oxidize and increase the oxygen content of the steel. The existing crystallizer wire feeding method exists Nozzle blockage and oxide layer problems.
It adopts rare earth iron alloy cored wire, the core is rare earth iron alloy (iron mass percentage 10-85wt.%, rare earth mass percentage 15-90wt.%), and the outer layer is low oxygen pure iron, low carbon steel or ultra-low carbon steel. Rare earth iron alloy powder is prepared under an inert atmosphere and coated with a protective layer to form a cored wire to increase the melting point and density and prevent oxidation and floating.
It effectively improves the yield and distribution uniformity of rare earths in steel, prevents oxidation and floating of rare earths, reduces the damage to the physical and chemical properties of protective slag, and improves the quality of steel.
Smart Images

Figure CN115896394B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel smelting, and in particular to a rare earth iron alloy cored wire and a preparation method thereof. Background Art
[0002] In the field of iron and steel metallurgy, rare earths can play a role in deoxidation and desulfurization, improving inclusion morphology and microalloying, and are therefore widely used in the production of high-quality steel. However, due to the relatively active nature of rare earths, the problem of low rare earth recovery in steel has always plagued the industry.
[0003] Han Yunlong and others used the method of in-ladle pressure injection instead of the injection method to add rare earth to steel, which increased the rare earth recovery rate from 7.0% to 22.1%. Xia Maosen and others used the method of feeding rare earth alloy wire in the ladle, controlling the process parameters such as argon blowing stirring intensity and feeding speed, and adding rare earth to the molten steel through a long conduit, so that the rare earth recovery rate reached 36.0%. The method of adding rare earth to the ladle is simple to operate, but the rare earth recovery rate is generally lower than 30%. Zhang Xuesong and others used the method of feeding rare earth wire in the tundish, and the rare earth recovery rate in the produced slabs was about 30%. When the rare earth wire was fed into the tundish, it would react with the covering agent, affecting the performance of the covering agent; in addition, the rare earth would react with the refractory material of the submerged long nozzle, causing the nozzle to be blocked by nodules. Yao Yongkuan and others compared the two methods of feeding wire in the tundish and feeding rare earth wire in the crystallizer, and found that the rare earth recovery rate of the ingot produced by the crystallizer wire feeding method was much higher than that of the ingot produced by the tundish wire feeding method; the study showed that the crystallizer wire feeding method is the most practical method to improve the rare earth recovery rate in steel. Zhao Chenglin and others achieved the purpose of further improving the rare earth recovery rate by adjusting the amount of rare earth wire added to the crystallizer, the wire feeding speed and the wire feeding position, and did not cause nozzle nodules, and the rare earth recovery rate was above 90%.
[0004] The wire feeding method is the most practical and mature method to improve the rare earth recovery rate in steel. However, there are some problems with the wire feeding method: (1) Pure rare earth has a low melting point and low density. After the rare earth enters the crystallizer, the rare earth and its generated inclusions tend to float up, affecting the physical and chemical properties of the protective slag, causing the surface quality of the ingot to deteriorate, resulting in a decrease in the rare earth recovery rate; (2) Rare earth metals are easily oxidized. During the preparation, packaging, storage and transportation of rare earth metal wires, rare earth metals come into contact with oxygen, resulting in a 100 μm thick oxide layer on the outer layer of the rare earth metal; these rare earth oxides have a high melting point, and when added to the crystallizer with the rare earth wire, they will seriously damage the role of the protective slag and increase the oxygen content of the steel; (3) Rare earth is fed into the crystallizer in the form of wires and cannot be homogenized in time, affecting the uniform distribution of rare earth in the steel. Summary of the invention
[0005] The purpose of the embodiment of the present invention is to provide a rare earth iron alloy cored wire and a preparation method thereof. The rare earth iron alloy cored wire can effectively prevent the oxidation of rare earth metals. Compared with pure rare earth, rare earth iron alloy has higher melting point and density, which solves the problem that rare earth and its inclusions are easy to float up after entering the crystallizer, affecting the physical and chemical properties of the protective slag, and effectively improves the rare earth yield and distribution uniformity of the finished steel product; in addition, there is no need to add other elements (such as calcium, silicon, aluminum, etc.), and no new impurities will be introduced, which is easy to promote and apply in industry.
[0006] In order to solve the above technical problems, a first aspect of an embodiment of the present invention provides a rare earth iron alloy cored wire, comprising: a core and a protective layer;
[0007] The core is a rare earth iron alloy, wherein the mass percentage of iron in the rare earth iron alloy is 10-85wt.%, and the mass percentage of rare earth is 15-90wt.%;
[0008] The protective layer is one of low-oxygen pure iron, low-carbon steel and ultra-low-carbon steel.
[0009] Furthermore, the mass percentage of iron in the rare earth iron alloy is 50-70wt.%, and the mass percentage of rare earth is 30-50wt.%.
[0010] Furthermore, the protective layer is low-oxygen pure iron.
[0011] Furthermore, the chemical composition of the iron includes, by mass percentage, C 0.0008-0.02%, Si 0.01-0.37%, Mn 0.02-0.65%, P 0.003-0.035%, S 0.003-0.035%, Cr 0.01-0.10%, Ni 0.01-0.30%, Cu 0.01-0.25%, Al≤0.05% and the balance Fe.
[0012] Further, the cross-sectional diameter of the core is Φ3.0-12.0 mm, and the thickness of the protective layer is 0.3-0.8 mm;
[0013] Preferably, the cross-sectional diameter of the core is Φ5.0-10.0 mm, and the thickness of the protective layer is 0.4-0.6 mm.
[0014] Further, the rare earth is at least one of lanthanum, cerium, praseodymium, neodymium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, lutetium, scandium and yttrium;
[0015] Preferably, the rare earth is at least one of lanthanum, cerium and yttrium.
[0016] The introduction of iron into the core of the rare earth iron alloy cored wire effectively improves the melting point, density and oxidizable properties of the core; secondly, crushing and powdering the rare earth iron alloy under an inert atmosphere can effectively prevent rare earth oxidation, and the preparation process is simpler than that of rare earth wire, and entering the molten steel in the form of powder is conducive to the uniform distribution of rare earth; in addition, a protective layer coated on the outer layer can further prevent rare earth oxidation and prevent rare earth from reacting with the crystallizer protective slag when entering the molten steel.
[0017] Accordingly, a second aspect of an embodiment of the present invention provides a method for preparing a rare earth iron alloy cored wire, comprising the following steps:
[0018] Step 1: preparing a rare earth iron alloy, placing a preset mass ratio of rare earth metal and pure iron into a crucible in a furnace body, closing the furnace cover and performing a vacuum operation, when the vacuum degree in the furnace drops to a first preset vacuum degree value, filling the furnace with an inert protective gas until the vacuum degree in the furnace reaches a second preset vacuum degree value, adjusting the heating power to heat step by step, when the melt temperature reaches the first preset temperature, keeping the temperature for a first preset time, and then casting, when the temperature in the furnace drops to room temperature, taking out the rare earth iron alloy;
[0019] Step 2: preparing rare earth iron alloy powder, grinding off the oxide layer of the rare earth iron alloy with a polisher under the protection of the inert protective gas, the grinding thickness being a first preset length, and then crushing the rare earth iron alloy with a crushing device, and screening the rare earth iron alloy powder with a vibrating screen after crushing, and packaging the rare earth iron alloy powder with a fineness not greater than the second preset length;
[0020] Step 3: preparing a rare earth iron alloy cored wire by using the rare earth iron alloy powder to prepare the rare earth iron alloy cored wire through a wire wrapping machine under the inert protective gas.
[0021] Furthermore, the first preset vacuum value is 0.1-1.0Pa;
[0022] The second preset vacuum value is 20-40 kPa.
[0023] Further, the first preset temperature is 1550-1700°C;
[0024] The first preset time length is 10-20 minutes.
[0025] Further, the first preset length is 30-80 μm;
[0026] The second preset length is less than or equal to 0.25 mm.
[0027] The above technical solution of the embodiment of the present invention has the following beneficial technical effects:
[0028] 1) The rare earth iron alloy in the core of the cored wire has a higher density and melting point than rare earth. Adding rare earth in the form of rare earth iron alloy can effectively avoid the rapid melting and floating of rare earth after entering the molten steel and the formation and floating of rare earth inclusions at a position close to the protective slag, which can effectively avoid the destruction of the physical and chemical properties of the protective slag.
[0029] 2) Rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0030] 3) The outer layer of the cored wire not only protects the core from rare earth oxidation, but also has a higher melting point, which can slow down the melting of the core when the cored wire enters the molten steel.
[0031] 4) The preparation of rare earth iron alloy, crushing and powdering, and cored wire under an inert atmosphere can effectively prevent rare earth oxidation and reduce the amount of rare earth oxides introduced into the molten steel during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a flow chart of a method for preparing a rare earth iron alloy cored wire provided in an embodiment of the present invention.
[0033] Figure 2 Schematic diagram of the distribution of sampling points on the cross section of the ingot according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0035] A first aspect of an embodiment of the present invention provides a rare earth iron alloy cored wire, comprising: a core and a protective layer; the core is a rare earth iron alloy, the mass percentage of iron in the rare earth iron alloy is 10-85wt.%, and the mass percentage of rare earth is 15-90wt.%; the protective layer is one of low-oxygen pure iron, low carbon steel, and ultra-low carbon steel.
[0036] Preferably, the mass percentage of iron in the rare earth iron alloy is 50-70wt.%, and the mass percentage of rare earth is 30-50wt.%.
[0037] Preferably, the protective layer is low-oxygen pure iron.
[0038] Specifically, the chemical composition of iron includes, by mass percentage, C 0.0008-0.02%, Si 0.01-0.37%, Mn 0.02-0.65%, P 0.003-0.035%, S 0.003-0.035%, Cr 0.01-0.10%, Ni 0.01-0.30%, Cu 0.01-0.25%, Al≤0.05% and the balance Fe.
[0039] Preferably, the cross-sectional diameter of the core is Φ3.0-12.0 mm, and the thickness of the protective layer is 0.3-0.8 mm; more preferably, the cross-sectional diameter of the core is Φ5.0-10.0 mm, and the thickness of the protective layer is 0.4-0.6 mm.
[0040] Specifically, the rare earth is at least one of lanthanum, cerium, praseodymium, neodymium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, lutetium, scandium and yttrium; preferably, the rare earth is at least one of lanthanum, cerium and yttrium.
[0041] The above-mentioned rare earth iron alloy cored wire has rare earth iron alloy powder as the core, and one of low-oxygen pure iron, low-carbon steel, and ultra-low carbon steel as the outer layer. In the core, the introduction of metallic iron effectively improves the melting point, density and oxidation resistance of the core rare earth. Secondly, the use of rare earth iron alloy powder can effectively solve the problem of uniform distribution of rare earth in steel, and the preparation process is simpler than that of rare earth wire. In addition, a protective layer coated on the outer layer can further prevent the oxidation of rare earth and prevent the rare earth from reacting with the crystallizer protective slag when entering the molten steel.
[0042] Accordingly, please refer to Figure 1 A second aspect of an embodiment of the present invention provides a method for preparing a rare earth iron alloy cored wire, comprising the following steps:
[0043] Step 1: preparing a rare earth iron alloy, placing a preset mass ratio of rare earth metal and pure iron into a crucible in a furnace body, closing the furnace cover and performing a vacuum operation, when the vacuum degree in the furnace drops to a first preset vacuum degree value, filling the furnace with an inert protective gas until the vacuum degree in the furnace reaches a second preset vacuum degree value, adjusting the heating power for step-by-step heating, when the melt temperature reaches the first preset temperature, keeping the temperature for a first preset time, and then casting, and when the temperature in the furnace drops to room temperature, taking out the rare earth iron alloy;
[0044] Step 2: preparing rare earth iron alloy powder, grinding off the oxide layer of the rare earth iron alloy with a polisher under the protection of an inert protective gas, the grinding thickness being a first preset length, and then crushing the rare earth iron alloy with a crushing device, and sieving the rare earth iron alloy powder with a vibrating screen after crushing, and packaging the rare earth iron alloy powder with a fineness not greater than a second preset length;
[0045] Step 3: preparing a rare earth iron alloy cored wire by using a wire wrapping machine under an inert protective gas and using rare earth iron alloy powder to prepare the rare earth iron alloy cored wire.
[0046] Optionally, the first preset vacuum degree value is 0.1-1.0 Pa; the second preset vacuum degree value is 20-40 kPa.
[0047] Optionally, the first preset temperature is 1550-1700°C; the first preset time is 10-20min.
[0048] Optionally, the first preset length is 30-80 μm; and the second preset length is less than or equal to 0.25 mm.
[0049] The following is a detailed description of the preparation process of the rare earth iron alloy cored wire using several embodiments:
[0050] Example 1
[0051] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0052] The preparation method of rare earth iron alloy cored wire is as follows:
[0053] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0054] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0055] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0056] The Ce-Fe alloy cored wire of this embodiment and the Ce cored wire with pure rare earth Ce wire as the core are fed into the crystallizer at the same wire feeding position and wire feeding speed using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Five points are evenly taken along the width direction at half of the thickness of the cross section of the billet, and samples are taken for rare earth content analysis. The specific locations of the sampling points are as follows: Figure 2 The test results are shown in Table 1.
[0057] The average rare earth recovery rate of Ce-Fe alloy cored wire is 97.5%, and the average rare earth recovery rate of Ce cored wire is 67.3%. The rare earth recovery rate of Ce-Fe alloy cored wire is 30.2% higher than that of Ce cored wire, which proves that the use of Ce-Fe alloy cored wire can significantly improve the rare earth recovery rate of steel. In addition, when using Ce-Fe alloy cored wire, the rare earth content of the five sampling points fluctuates within 3ppm and is evenly distributed. When using rare earth cored wire, the rare earth distribution of the five sampling points is uneven, with the maximum difference of 24ppm. This also proves that rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0058] Table 1 Test results of rare earth content in steel
[0059]
[0060] Example 2
[0061] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 10wt.%, Ce 90wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low carbon steel, and its thickness is 0.5mm;
[0062] The preparation method of rare earth iron alloy cored wire is as follows:
[0063] (1) Place 15kg of pure iron and 135kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0064] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0065] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0066] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 94.5%, and the rare earth content of the five sampling points fluctuates within 5ppm and is evenly distributed.
[0067] Example 3
[0068] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 50wt.%, Ce 50wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is ultra-low carbon steel, and its thickness is 0.5mm;
[0069] The preparation method of rare earth iron alloy cored wire is as follows:
[0070] (1) Place 75kg of pure iron and 75kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0071] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0072] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0073] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 96.6%, and the rare earth content of the five sampling points fluctuates within 4ppm and is evenly distributed.
[0074] Example 4
[0075] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 70wt.%, Ce 30wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0076] The preparation method of rare earth iron alloy cored wire is as follows:
[0077] (1) Place 105kg of pure iron and 45kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0078] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0079] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0080] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 95.4%, and the rare earth content of the five sampling points fluctuates within 4ppm and is evenly distributed.
[0081] Example 5
[0082] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 85wt.%, Ce 15wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0083] The preparation method of rare earth iron alloy cored wire is as follows:
[0084] (1) Place 127.5 kg of pure iron and 22.5 kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5 Pa, fill the furnace with argon until the vacuum in the furnace reaches 30 kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600 ° C, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0085] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0086] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0087] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 94.2%, and the rare earth content of the five sampling points fluctuates within 6ppm and is evenly distributed.
[0088] Example 6
[0089] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, La 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0090] The preparation method of rare earth iron alloy cored wire is as follows:
[0091] (1) Place 90kg of pure iron and 60kg of La into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.1Pa, fill the furnace with argon until the vacuum in the furnace reaches 20kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1550℃, keep it warm for 10 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the La-Fe alloy;
[0092] (2) The La-Fe alloy as described in (1) is polished off by a polishing machine under the protection of an inert protective gas by 70 μm, and then the La-Fe alloy is crushed and powdered. The fineness of the La-Fe alloy powder is 0.08-0.25 mm;
[0093] (3) Using a wire wrapping machine under the protection of an inert protective gas, the La-Fe alloy powder described in (2) is used to prepare a La-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the La-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0094] The La-Fe alloy cored wire of this embodiment and the La cored wire with the core being pure rare earth La wire were respectively fed into the crystallizer at the same wire feeding position and wire feeding speed using a wire feeder, and finally a rare earth steel continuous casting billet was obtained. The same test method and sampling point as in Example 1 were used, and the test results are shown in Table 2.
[0095] The average rare earth recovery rate of La-Fe alloy cored wire is 93%, and the average rare earth recovery rate of La cored wire is 69%. The rare earth recovery rate of La-Fe alloy cored wire is 24% higher than that of La cored wire, which proves that the use of La-Fe alloy cored wire can significantly improve the rare earth recovery rate of steel. In addition, when using La-Fe alloy cored wire, the rare earth content of the five sampling points fluctuates within 5ppm and is evenly distributed. When using rare earth cored wire, the rare earth distribution of the five sampling points is uneven, with the maximum difference of 35ppm. This also proves that rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0096] Table 2 Test results of rare earth content in steel
[0097]
[0098]
[0099] Example 7
[0100] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Y 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0101] The preparation method of rare earth iron alloy cored wire is as follows:
[0102] (1) Place 90kg of pure iron and 60kg of Y into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 1Pa, fill the furnace with argon until the vacuum in the furnace reaches 40kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1650℃, keep it warm for 20 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Y-Fe alloy;
[0103] (2) The Y-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 50 μm, and then the Y-Fe alloy is crushed and powdered. The fineness of the Y-Fe alloy powder is 0.08-0.25 mm;
[0104] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Y-Fe alloy powder described in (2) is used to prepare a Y-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Y-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0105] The Y-Fe alloy cored wire of this embodiment and the Y cored wire with the core of pure rare earth Y wire were fed into the crystallizer at the same wire feeding position and wire feeding speed using a wire feeder, and finally a rare earth steel continuous casting billet was obtained. The same test method and sampling point as in Example 1 were used, and the test results are shown in Table 3.
[0106] The average rare earth recovery rate of Y-Fe alloy cored wire is 94.5%, and the average rare earth recovery rate of Y cored wire is 66.9%. The rare earth recovery rate of Y-Fe alloy cored wire is 27.6% higher than that of Y cored wire, which proves that the use of Y-Fe alloy cored wire can significantly improve the rare earth recovery rate of steel. In addition, when using Y-Fe alloy cored wire, the rare earth content of the five sampling points fluctuates within 5ppm and is evenly distributed. When using rare earth cored wire, the rare earth distribution of the five sampling points is uneven, with the maximum difference of 21ppm. This also proves that rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0107] Table 3 Test results of rare earth content in steel
[0108]
[0109] Example 8
[0110] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Nd 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0111] The preparation method of rare earth iron alloy cored wire is as follows:
[0112] (1) Place 90kg of pure iron and 60kg of Nd into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.25Pa, fill the furnace with argon until the vacuum in the furnace reaches 25kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1570℃, keep it warm for 13 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Nd-Fe alloy;
[0113] (2) The Nd-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 40 μm, and then the Nd-Fe alloy is crushed and powdered. The fineness of the Nd-Fe alloy powder is 0.08-0.25 mm;
[0114] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Nd-Fe alloy powder described in (2) is used to prepare a Nd-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the obtained Nd-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0115] The Nd-Fe alloy cored wire of this embodiment and the Nd cored wire with the core of pure rare earth Nd wire were fed into the crystallizer at the same wire feeding position and wire feeding speed using a wire feeder, and finally a rare earth steel continuous casting billet was obtained. The same test method and sampling point as in Example 1 were used, and the test results are shown in Table 4.
[0116] The average rare earth recovery rate of Nd-Fe alloy cored wire is 92.8%, and the average rare earth recovery rate of Nd cored wire is 70.7%. The rare earth recovery rate of Nd-Fe alloy cored wire is 22.1% higher than that of Nd cored wire, which proves that the use of Nd-Fe alloy cored wire can significantly improve the rare earth recovery rate of steel. In addition, when using Nd-Fe alloy cored wire, the rare earth content of the five sampling points fluctuates within 6ppm and is evenly distributed. When using rare earth cored wire, the rare earth distribution of the five sampling points is uneven, with the maximum difference of 23ppm. This also proves that rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0117] Table 4 Test results of rare earth content in steel
[0118]
[0119] Example 9
[0120] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Pr 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0121] The preparation method of rare earth iron alloy cored wire is as follows:
[0122] (1) Place 90kg of pure iron and 60kg of Pr into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum degree in the furnace drops to 0.75Pa, fill the furnace with argon until the vacuum degree in the furnace is 35kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1700℃, keep it warm for 16 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Pr-Fe alloy;
[0123] (2) The Pr-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 30 μm, and then the Pr-Fe alloy is crushed and powdered. The fineness of the Pr-Fe alloy powder is 0.08-0.25 mm;
[0124] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Pr-Fe alloy powder described in (2) is used to prepare a Pr-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Pr-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0125] The Pr-Fe alloy cored wire of this embodiment and the Pr cored wire with pure rare earth Pr wire as the core are respectively fed into the crystallizer at the same wire feeding position and wire feeding speed by a wire feeder, and finally a rare earth steel continuous casting billet is obtained. The same test method and sampling point as in Example 1 are used, and the test results are shown in Table 5.
[0126] The average rare earth recovery rate of Pr-Fe alloy cored wire is 93.1%, and the average rare earth recovery rate of Pr cored wire is 72.7%. The rare earth recovery rate of Pr-Fe alloy cored wire is 20.4% higher than that of Pr cored wire, which proves that the use of Pr-Fe alloy cored wire can significantly improve the rare earth recovery rate of steel. In addition, when using Pr-Fe alloy cored wire, the rare earth content of the five sampling points fluctuates within 8ppm and is evenly distributed. When using rare earth cored wire, the rare earth distribution of the five sampling points is uneven, with the maximum difference of 29ppm. This also proves that rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel.
[0127] Table 5 Test results of rare earth content in steel
[0128]
[0129] Example 10
[0130] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.3mm;
[0131] The preparation method of rare earth iron alloy cored wire is as follows:
[0132] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0133] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0134] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.3 mm.
[0135] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 95.2%, and the rare earth content of the five sampling points fluctuates within 7ppm and is evenly distributed.
[0136] Embodiment 11
[0137] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.4mm;
[0138] The preparation method of rare earth iron alloy cored wire is as follows:
[0139] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0140] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0141] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.4 mm.
[0142] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 96.6%, and the rare earth content of the five sampling points fluctuates within 3ppm and is evenly distributed.
[0143] Example 12
[0144] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.6mm;
[0145] The preparation method of rare earth iron alloy cored wire is as follows:
[0146] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0147] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0148] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.6 mm.
[0149] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 96.8%, and the rare earth content of the five sampling points fluctuates within 3ppm and is evenly distributed.
[0150] Embodiment 13
[0151] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer in the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ8.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.8mm;
[0152] The preparation method of rare earth iron alloy cored wire is as follows:
[0153] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0154] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0155] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ8.0 mm; the thickness of the outer protective layer is 0.8 mm.
[0156] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 94.6%, and the rare earth content of the five sampling points fluctuates within 8ppm and is evenly distributed.
[0157] Embodiment 14
[0158] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer in the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ3.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0159] The preparation method of rare earth iron alloy cored wire is as follows:
[0160] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0161] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0162] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ3.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0163] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 94.8%, and the rare earth content of the five sampling points fluctuates within 6ppm and is evenly distributed.
[0164] Embodiment 15
[0165] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer in the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ5.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0166] The preparation method of rare earth iron alloy cored wire is as follows:
[0167] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0168] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0169] (3) Using a wire wrapping machine under the protection of an inert gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ5.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0170] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 96.9%, and the rare earth content of the five sampling points fluctuates within 4ppm and is evenly distributed.
[0171] Example 16
[0172] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer on the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ10.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0173] The preparation method of rare earth iron alloy cored wire is as follows:
[0174] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0175] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0176] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ10.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0177] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 96.4%, and the rare earth content of the five sampling points fluctuates within 5ppm and is evenly distributed.
[0178] Embodiment 17
[0179] The rare earth iron alloy cored wire is composed of rare earth iron alloy powder in the core and a protective layer in the outer layer; the composition of the rare earth iron alloy powder in the core is: Fe 60wt.%, Ce 40wt.%, the fineness of the rare earth iron alloy powder is 0.08-0.25mm, and the core diameter of the rare earth iron alloy cored wire is Φ12.0mm; the outer protective layer is low-oxygen pure iron, and its thickness is 0.5mm;
[0180] The preparation method of rare earth iron alloy cored wire is as follows:
[0181] (1) Place 90kg of pure iron and 60kg of Ce into a crucible in a smelting furnace, close the furnace cover, and use a mechanical pump and a Roots pump to evacuate the furnace. When the vacuum in the furnace drops to 0.5Pa, fill the furnace with argon until the vacuum in the furnace reaches 30kPa. Then, adjust the heating power and heat step by step. When the melt temperature reaches 1600℃, keep it warm for 15 minutes and then cast it. When the temperature in the furnace drops to room temperature, take out the Ce-Fe alloy;
[0182] (2) The Ce-Fe alloy as described in (1) is polished by a polishing machine under the protection of an inert protective gas to remove 80 μm, and then the Ce-Fe alloy is crushed and powdered. The fineness of the Ce-Fe alloy powder is 0.08-0.25 mm;
[0183] (3) Using a wire wrapping machine under the protection of an inert protective gas, the Ce-Fe alloy powder described in (2) is used to prepare a Ce-Fe alloy cored wire. Finally, the cross-sectional diameter of the core of the Ce-Fe alloy cored wire is Φ12.0 mm; the thickness of the outer protective layer is 0.5 mm.
[0184] The Ce-Fe alloy cored wire of this embodiment is fed into the crystallizer using a wire feeder, and finally a rare earth steel continuous casting billet is obtained. Using the same test method as in Example 1, the average rare earth recovery rate of the Ce-Fe alloy cored wire of this embodiment is measured to be 95.1%, and the rare earth content of the five sampling points fluctuates within 9ppm and is evenly distributed.
[0185] The above preparation process and working principle are as follows: rare earth and iron are pre-melted together in a certain proportion to form a rare earth iron alloy, and then crushed and powdered under an inert atmosphere. Finally, the rare earth iron alloy powder is used as the core and the protective layer is wrapped to prepare a rare earth iron alloy cored wire. Due to the low melting point of rare earth, pure rare earth will melt quickly after entering the crystallizer. A part of the rare earth will float up and react with the protective slag due to density and other reasons. In addition, since the rare earth melts quickly after entering the molten steel, rare earth inclusions will be generated at a position close to the protective slag, and these inclusions are also easy to float, thereby affecting the physical and chemical properties of the protective slag. Rare earth iron alloy has a higher density and melting point than rare earth. Adding rare earth in the form of rare earth iron alloy can effectively avoid the rapid melting and floating of rare earth after entering the molten steel and the generation and floating of rare earth inclusions at a position close to the protective slag, which can effectively avoid the destruction of the physical and chemical properties of the protective slag. The preparation of rare earth iron alloy, crushing and powdering, and preparation of cored wire under inert atmosphere can effectively prevent rare earth oxidation and reduce the amount of rare earth oxides introduced. Secondly, the rare earth iron alloy enters the molten steel in the form of powder, which can make the rare earth elements more evenly distributed in the steel. In addition, the outer protective layer is low-oxygen pure iron or low-carbon steel or ultra-low-carbon steel, which can not only protect the core from rare earth oxidation, but also has a high melting point, which can slow down the melting of the core when the cored wire enters the molten steel.
[0186] In summary, the present invention aims at the many problems existing in feeding rare earth wire into the crystallizer to improve the performance of steel during the steel smelting process. The present invention introduces iron with high melting point and density into the core material of the cored wire, pre-melts the rare earth metal and iron, crushes and powders them, and finally forms a rare earth iron alloy cored wire with an outer protective layer. Starting from the four aspects of melting point, density, antioxidant capacity and dispersibility, this patent solves the problem that when pure rare earth wire is fed into the crystallizer, the rare earth and its generated inclusions are easy to float up and affect the physical and chemical properties of the protective slag, resulting in low rare earth recovery rate and uniform rare earth distribution, and develops a rare earth iron alloy cored wire and its preparation method.
[0187] The embodiment of the present invention aims to protect a rare earth iron alloy cored wire, comprising: a core and a protective layer; the core is a rare earth iron alloy, the mass percentage of iron in the rare earth iron alloy is 10-85wt.%, and the mass percentage of rare earth is 15-90wt.%; the protective layer is one of low-oxygen pure iron, low-carbon steel, and ultra-low-carbon steel. The above technical solution has the following effects:
[0188] A rare earth iron alloy cored wire is prepared with rare earth iron alloy powder as the core and one of low-oxygen pure iron, low-carbon steel and ultra-low carbon steel as the outer layer. The rare earth metal and iron are pre-melted together to effectively prevent rare earth oxidation, reduce the introduction of rare earth oxides, and improve the melting point and density of the material. During use, it can effectively prevent rare earth metals and their inclusions from floating up and reacting with protective slag to affect the properties of the protective slag, thereby improving the rare earth recovery rate in the finished steel product and the uniformity of rare earth distribution in the steel.
[0189] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A rare earth iron alloy cored wire, It is characterized in that include: core and protective layer; The core is a rare earth iron alloy, wherein the mass percentage of iron in the rare earth iron alloy is 10-50wt.%, and the mass percentage of rare earth is 50-90wt.%; The protective layer is one of low-oxygen pure iron, low-carbon steel and ultra-low carbon steel; The chemical composition of the iron includes, by mass percentage, C 0.0008-0.02%, Si 0.01-0.37%, Mn 0.02-0.65%, P 0.003-0.035%, S 0.003-0.035%, Cr 0.01-0.10%, Ni 0.01-0.30%, Cu 0.01-0.25%, Al≤0.05% and the balance Fe; The cross-sectional diameter of the core is Φ 3.0-12.0 mm, and the thickness of the protective layer is 0.3-0.8 mm.
2. The rare earth iron alloy cored wire according to claim 1, It is characterized in that The cross-sectional diameter of the core is Φ 5.0-10.0 mm, and the thickness of the protective layer is 0.4-0.6 mm.
3. The rare earth iron alloy cored wire according to claim 1 or 2, It is characterized in that The rare earth is at least one of lanthanum, cerium, praseodymium, neodymium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, lutetium, scandium and yttrium.
4. A method for preparing a rare earth iron alloy cored wire as claimed in any one of claims 1 to 3, It is characterized in that The steps include: Step 1: preparing a rare earth iron alloy, placing a preset mass ratio of rare earth metal and iron into a crucible in a furnace body, closing the furnace cover and performing a vacuum operation, when the vacuum degree in the furnace drops to a first preset vacuum degree value, filling the furnace with an inert protective gas until the vacuum degree in the furnace reaches a second preset vacuum degree value, adjusting the heating power to heat step by step, when the melt temperature reaches the first preset temperature, keeping the temperature for a first preset time, and then casting, when the temperature in the furnace drops to room temperature, taking out the rare earth iron alloy; Step 2: preparing rare earth iron alloy powder, grinding off the oxide layer of the rare earth iron alloy with a polisher under the protection of the inert protective gas, the grinding thickness being a first preset length, and then crushing the rare earth iron alloy with a crushing device, and sieving the rare earth iron alloy powder with a vibrating screen after crushing, and packaging the rare earth iron alloy powder with a fineness not greater than the second preset length; Step 3: preparing a rare earth iron alloy cored wire by using the rare earth iron alloy powder to prepare the rare earth iron alloy cored wire through a wire wrapping machine under the inert protective gas.
5. The method for preparing the rare earth iron alloy cored wire according to claim 4, It is characterized in that The first preset vacuum value is 0.1-1.0 Pa; The second preset vacuum value is 20-40 kPa.
6. The method for preparing the rare earth iron alloy cored wire according to claim 4, It is characterized in that The first preset temperature is 1550-1700°C; The first preset time length is 10-20 minutes.
7. The method for preparing the rare earth iron alloy cored wire according to claim 4, It is characterized in that The first preset length is 30-80 μm; The second preset length is less than or equal to 0.25 mm.
Citation Information
Patent Citations
Fe-La intermediate alloy for rare earth addition into steel and manufacture method thereof
CN102373360A
Preparation method of rare earth-iron intermediate alloy for low-oxygen rare earth steel
CN106756446A
Preparation method of low-oxygen high-purity rare earth alloy
CN111962102A
High-strength microalloyed rare-earth cast steel
WO2018018389A1
Rare-earth microalloyed steel and control method
WO2021046937A1
Cited By
Active metal iron alloy cored wire and preparation method thereof
CN122484399A